Preparation method of bio-based thermoplastic polyurethane elastomer
By introducing quaternized rosinate chain extender into bio-based thermoplastic polyurethane elastomers, combining the polymerization reaction of polyols and diisocyanates, the problems of insufficient heat resistance and antibacterial properties of polyurethane elastomers are solved, and a higher level of Mechanical properties and thermal decomposition temperature, and have good antibacterial effects.
Patent Information
- Application Number
- CN202411562151.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-05
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-11-05
AI Technical Summary
The existing bio-based thermoplastic polyurethane elastomers have shortcomings in terms of heat resistance and antibacterial properties, and have failed to effectively solve the problems of poor heat resistance and lack of antibacterial properties of polyurethane elastomers.
The quaternized rosinate chain extender is used to polymerize with polyols and diisocyanate. The hydrogenated triphenyl ring structure and quaternary ammonium salt groups are introduced through esterification and substitution reactions to form a biomass with high structural stability and antibacterial properties. Thermoplastic polyurethane elastomer.
It significantly improves the tensile strength, elongation of break and thermal decomposition temperature of polyurethane elastomers, enhances heat resistance, and shows good antibacterial properties, which can effectively inhibit bacterial growth.
Smart Images

Figure SMS_9 
Figure SMS_10 
Figure QLYQS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyurethane elastomers, in particular to a method for preparing a bio-based thermoplastic polyurethane elastomer. Background Art
[0002] Polyurethane elastomers have good wear resistance, elasticity and impact resistance, and are widely used in footwear, sports equipment, medical equipment, etc. The development of green and environmentally friendly bio-based polyurethane materials is a research hotspot. Polyurethane materials prepared using biomass resources such as lignin, cellulose, and natural oils as raw materials have the characteristics of being green, biodegradable, and having excellent mechanical properties.
[0003] Rosin acid is one of the main components of rosin. It is widely found in pine and other plants. It is a cheap and easily available green and environmentally friendly bio-based resource. It is widely used in polymer materials such as plastics and rubbers to improve the heat resistance and waterproof properties of materials. The patent with the authorization announcement number CN114133517B discloses a rosin-based polyurethane and its synthesis method. Rosin anhydride is subjected to imidization reaction, chlorination reaction, and esterification reaction in sequence to obtain rosin-based polyol; then reacted with diisocyanate, the obtained rosin-based polyurethane has good mechanical and thermal stability. However, the rosin-based polyurethane of the patent does not show antibacterial properties. Summary of the invention
[0004] The technical problem solved by the present invention is: providing a method for preparing a bio-based thermoplastic polyurethane elastomer, solving the problem that the polyurethane elastomer has poor heat resistance and no antibacterial property.
[0005] The technical scheme adopted by the present invention is: a method for preparing a bio-based thermoplastic polyurethane elastomer, comprising the following steps: adding dried and dehydrated polyol and diisocyanate to a reaction bottle, stirring and reacting at 70-80°C for 2-3h, then adding a quaternized rosin ester chain extender, stirring to form a gel, then adding the mixture to a mold at a temperature of 100-110°C, placing the mixture for 1-1.5h, demolding the mixture and placing the mixture in a heating box, and ripening the mixture at 110-120°C for 18-24h to obtain the bio-based thermoplastic polyurethane elastomer; The structural formula of the quaternized rosin acid ester chain extender is as follows: , n is any integer from 2 to 8.
[0006] Preferably, the molar ratio of the polyol, diisocyanate and quaternized rosin ester chain extender is 1:(2.2-2.4):(1-1.2).
[0007] Preferably, the polyol is polytetramethylene ether diol, polybutylene adipate diol or polycaprolactone diol; and the diisocyanate is 4,4'-methylenebis(phenyl isocyanate) or toluene-2,4-diisocyanate.
[0008] Preferably, the preparation method of the quaternized rosin acid ester chain extender is: Step (1), add rosin acid, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, and 4-dimethylaminopyridine to N,N-dimethylformamide, stir and activate at room temperature for 20-40 minutes, then add diethanolamine, stir and react for 12-18 hours, transfer the solution to a separatory funnel, add water and ethyl acetate, shake and let stand to separate, dry the organic layer with anhydrous sodium sulfate to remove water, and recrystallize the filtrate to obtain a rosin acid ester intermediate. The reaction formula is: ; Step (2), add rosin acid ester intermediate, bromohydrin compound and potassium carbonate to acetonitrile, carry out substitution reaction at 40-50°C for 4-6h, then add bromohydrin compound, carry out quaternization reaction at 80-85°C for 12-18h under condensation reflux, distill under reduced pressure, add the product after washing with water to a mixed solution of ethanol and ethyl acetate, and recrystallize to obtain quaternized rosin acid ester chain extender. The reaction formula is: .
[0009] Preferably, in step (1), the molar ratio of rosin acid, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, 4-dimethylaminopyridine and diethanolamine is (2-2.2):(2.2-2.4):(0.14-0.18):1.
[0010] Preferably, in step (2), the molar ratio of the rosin acid ester intermediate, the bromohydrin compound and potassium carbonate is 1:(2-2.4):(2-2.2).
[0011] Preferably, the structural formula of the bromohydrin compound is , n is any integer from 2 to 8.
[0012] The beneficial effects of the present invention are as follows: the present invention uses rosin acid as an environmentally friendly bio-based material, performs an esterification reaction with diethanolamine, and then performs a substitution and quaternization reaction with a bromohydrin compound to obtain a novel quaternized rosin acid ester chain extender for polyurethane, and performs a polymerization chain extension reaction with polyols and diisocyanates to obtain a novel bio-based thermoplastic polyurethane elastomer.
[0013] The invention introduces a hydrogenated triphenanthrene ring structure with high structural stability and strong heat resistance and a quaternary ammonium salt group with antibacterial properties into a polyurethane elastomer, thereby improving the tensile strength and elongation at break of the elastomer and showing higher mechanical properties. At the same time, the thermal decomposition temperature and the diameter of the inhibition zone of the elastomer material are improved, and the elastomer has better heat resistance and antibacterial properties. DETAILED DESCRIPTION
[0014] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0015] Example 1: Preparation method of bio-based thermoplastic polyurethane elastomer: (1) Add 40 mmol of rosin acid, 44 mmol of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, and 3.6 mmol of 4-dimethylaminopyridine to N,N-dimethylformamide, stir and activate at room temperature for 30 minutes, then add 20 mmol of diethanolamine, stir and react for 18 hours, transfer the solution to a separatory funnel, add water and ethyl acetate, shake and let stand to separate, dry the organic layer with anhydrous sodium sulfate to remove water, and recrystallize the filtrate to obtain a rosin acid ester intermediate. The structural formula is: ; (2) Add 40 mmol of rosin acid ester intermediate, 42 mmol of 4-bromo-1-butanol, and 88 mmol of potassium carbonate to acetonitrile, carry out substitution reaction at 45°C for 4 hours, then add 44 mmol of 4-bromo-1-butanol, carry out quaternization reaction at 80°C for 18 hours under condensation reflux, distill under reduced pressure, add the product after washing with water to a mixed solution of ethanol and ethyl acetate, and recrystallize to obtain a quaternized rosin acid ester chain extender. The structural formula is: ; (3) Add 40 mmol of dried and dehydrated polybutylene adipate diol 2000 and 92 mmol of 4,4'-methylenebis(phenyl isocyanate) into the reaction bottle, stir and react at 75°C for 3 h, then add 44 mmol of quaternary ammonium rosin ester chain extender, stir to form a gel, then add to a mold at a temperature of 100°C, leave for 1.5 h, demold and place in a heating box, and mature at 110°C for 24 h to obtain a bio-based thermoplastic polyurethane elastomer.
[0016] Example 2: Preparation method of bio-based thermoplastic polyurethane elastomer: (1) Add 44 mmol of rosin acid, 48 mmol of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, and 3 mmol of 4-dimethylaminopyridine to N,N-dimethylformamide, stir and activate at room temperature for 20 min, then add 20 mmol of diethanolamine, stir and react for 18 h, transfer the solution to a separatory funnel, add water and ethyl acetate, shake and let stand to separate, dry the organic layer with anhydrous sodium sulfate to remove water, and recrystallize the filtrate to obtain a rosin acid ester intermediate; (2) Add 40 mmol of rosin acid ester intermediate, 40 mmol of 2-bromoethanol and 80 mmol of potassium carbonate to acetonitrile, carry out substitution reaction at 50°C for 5 hours, then add 40 mmol of 2-bromoethanol, carry out quaternization reaction at 85°C under condensation reflux for 18 hours, distill under reduced pressure, wash the product with water, add it to a mixed solution of ethanol and ethyl acetate, and recrystallize it to obtain a quaternized rosin acid ester chain extender; (3) Add 40 mmol of dried and dehydrated polytetramethylene ether diol 2000 and 96 mmol of 4,4'-methylenebis(phenyl isocyanate) into the reaction bottle, stir and react at 70°C for 3 h, then add 48 mmol of quaternary ammonium rosin ester chain extender and stir to form a gel. Then add it to a mold at a temperature of 110°C and leave it for 1 h. After demolding, place it in a heating box and mature it at 120°C for 18 h to obtain a bio-based thermoplastic polyurethane elastomer.
[0017] Example 3: Preparation method of bio-based thermoplastic polyurethane elastomer: (1) Add 44 mmol of rosin acid, 48 mmol of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, and 2.8 mmol of 4-dimethylaminopyridine to N,N-dimethylformamide, stir and activate at room temperature for 40 min, then add 20 mmol of diethanolamine, stir and react for 12 h, transfer the solution to a separatory funnel, add water and ethyl acetate, shake and let stand to separate, dry the organic layer with anhydrous sodium sulfate to remove water, and recrystallize the filtrate to obtain a rosin acid ester intermediate; (2) Add 40 mmol of rosin acid ester intermediate, 44 mmol of 8-bromo-1-octanol, and 88 mmol of potassium carbonate to acetonitrile, carry out substitution reaction at 50°C for 4 hours, then add 52 mmol of 8-bromo-1-octanol, carry out quaternization reaction at 80°C for 12 hours under condensation reflux, distill under reduced pressure, add the product after washing with water into a mixed solution of ethanol and ethyl acetate, and recrystallize to obtain a quaternized rosin acid ester chain extender; (3) Add 40 mmol of dried and dehydrated polycaprolactone diol 2000 and 88 mmol of toluene-2,4-diisocyanate into the reaction bottle, stir and react at 80°C for 2 h, then add 40 mmol of quaternary ammonium rosin ester chain extender, stir to form a gel, then add it to a mold at a temperature of 100°C, leave it for 1.5 h, demold it, place it in a heating box, and mature it at 120°C for 24 h to obtain a bio-based thermoplastic polyurethane elastomer.
[0018] Example 4: Preparation method of bio-based thermoplastic polyurethane elastomer: (1) Add 42 mmol of rosin acid, 48 mmol of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, and 3.2 mmol of 4-dimethylaminopyridine to N,N-dimethylformamide, stir and activate at room temperature for 20 min, then add 20 mmol of diethanolamine, stir and react for 18 h, transfer the solution to a separatory funnel, add water and ethyl acetate, shake and let stand to separate, dry the organic layer with anhydrous sodium sulfate to remove water, and recrystallize the filtrate to obtain a rosin acid ester intermediate; (2) Add 40 mmol of rosin acid ester intermediate, 40 mmol of 6-bromo-1-hexanol and 84 mmol of potassium carbonate to acetonitrile, carry out substitution reaction at 40°C for 6 hours, then add 44 mmol of 6-bromo-1-hexanol, carry out quaternization reaction at 85°C for 12 hours under condensation reflux, distill under reduced pressure, add the product after washing with water into a mixed solution of ethanol and ethyl acetate, and recrystallize to obtain a quaternized rosin acid ester chain extender; (3) Add 40 mmol of dried and dehydrated polytetramethylene glycol 2000 and 92 mmol of toluene-2,4-diisocyanate into the reaction bottle, stir and react at 75°C for 3 h, then add 44 mmol of quaternary ammonium rosin ester chain extender, stir to form a gel, then add it to a mold at a temperature of 100°C, leave it for 1.5 h, demold it, place it in a heating box, and mature it at 120°C for 18 h to obtain a bio-based thermoplastic polyurethane elastomer.
[0019] Comparative Example 1: Preparation method of thermoplastic polyurethane elastomer: (1) Add 40 mmol of dried and dehydrated polybutylene adipate diol 2000 and 92 mmol of 4,4'-methylenebis(phenyl isocyanate) into a reaction bottle, stir and react at 75°C for 3 h, then add 44 mmol of 1,4-butanediol and stir to form a gel. Then add the mixture into a mold at 100°C and leave it for 1.5 h. After demolding, place it in a heating box and mature it at 110°C for 24 h to obtain a thermoplastic polyurethane elastomer.
[0020] Comparative Example 2: Preparation method of bio-based thermoplastic polyurethane elastomer: (1) Add 40 mmol benzoic acid, 44 mmol 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, and 3.6 mmol 4-dimethylaminopyridine to N,N-dimethylformamide, stir and activate for 30 min at room temperature, then add 20 mmol diethanolamine, stir and react for 18 h, transfer the solution to a separatory funnel, add water and ethyl acetate, shake and let stand to separate, dry the organic layer with anhydrous sodium sulfate to remove water, and recrystallize the filtrate to obtain a benzoate intermediate. The structural formula is: ; (2) Add 40 mmol of benzoate intermediate, 42 mmol of 4-bromo-1-butanol, and 88 mmol of potassium carbonate to acetonitrile, carry out substitution reaction at 45°C for 4 hours, then add 44 mmol of 4-bromo-1-butanol, carry out quaternization reaction at 80°C for 18 hours under condensation reflux, distill under reduced pressure, add the product after washing with water to a mixed solution of ethanol and ethyl acetate, and recrystallize to obtain a quaternized benzoate chain extender. The structural formula is: ; (3) Add 40 mmol of dried and dehydrated polybutylene adipate diol 2000 and 92 mmol of 4,4'-methylenebis(phenyl isocyanate) into the reaction bottle, stir and react at 75°C for 3 h, then add 44 mmol of quaternary ammonium benzoate chain extender and stir to form a gel. Then add the mixture into a mold at a temperature of 100°C and leave it for 1.5 h. After demolding, place it in a heating box and mature it at 110°C for 24 h to obtain a bio-based thermoplastic polyurethane elastomer.
[0021] The cured polyurethane elastomer was placed at room temperature for 7 days. The tensile stress-strain properties were tested according to GB / T 528-2009.
[0022] The polyurethane elastomer was placed in a thermogravimetric analyzer for thermal performance analysis in a nitrogen atmosphere with a heating rate of 10°C / min and a test temperature of 25-700°C.
[0023] Table 1: Test results of various embodiments and comparative examples
[0024] T 5% is the temperature at which the mass loss is 5%. max is the temperature at which the rate of thermal weight loss is maximum.
[0025] The polyurethane elastomer was cut into sheets and pressed into a polyurethane film with a thickness of 1 mm; sterilized under ultraviolet light. Escherichia coli, Staphylococcus aureus and Candida albicans were activated at 37°C for 24 h and gradiently diluted to a concentration of 10 7cfu / mL bacterial suspension. Then, 0.1 mL of bacterial suspension was transferred to the surface of beef extract peptone agar medium, and then the polyurethane film was attached to the surface of the medium, placed in a constant temperature incubator, cultured at 37 for 24 hours, and the diameter of the inhibition zone was measured. Each group of film samples was tested 5 times and the average value was taken.
[0026] Table 2: Test results of various embodiments and comparative examples
[0027] After testing, the tensile strength and elongation at break of the polyurethane elastomer material obtained in Comparative Example 1 using 1,4-butanediol as a chain extender are low, and T 5% and T max It is low, has poor heat resistance, does not contain quaternary ammonium salt groups, has no antibacterial properties, and does not show an inhibition zone diameter.
[0028] Example 1-Example 4 Utilize quaternized rosin acid ester chain extender, introduce hydrogenated triphenanthrene ring structure with high structural stability and strong heat resistance, and antibacterial quaternary ammonium salt group into polyurethane elastomer, significantly improve the tensile strength and elongation at break of elastomer, and have higher thermal decomposition temperature and better heat resistance. And have good antibacterial property, and show high inhibition zone diameter to bacteria such as Escherichia coli.
[0029] In Comparative Example 2, benzoic acid, diethanolamine and 4-bromo-1-butanol were used as reactants to prepare a quaternary ammonium benzoate chain extender. The prepared polyurethane elastomer material did not contain a hydrogenated triphenanthrene ring structure, and the tensile strength, elongation at break and thermal decomposition temperature of the elastomer were low.
[0030] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a bio-based thermoplastic polyurethane elastomer, characterized in that: The method comprises the following steps: adding dried and dehydrated polyol and diisocyanate into a reaction bottle, stirring and reacting at 70-80°C for 2-3h, then adding a quaternized rosin acid ester chain extender, stirring to form a gel, then adding the mixture into a mold at a temperature of 100-110°C, placing the mixture for 1-1.5h, demolding the mixture, placing the mixture in a heating box, and ripening the mixture at 110-120°C for 18-24h to obtain a bio-based thermoplastic polyurethane elastomer; The structural formula of the quaternized rosin acid ester chain extender is as follows: , n is any integer from 2 to 8.
2. The method for preparing a bio-based thermoplastic polyurethane elastomer according to claim 1, characterized in that: The molar ratio of the polyol, diisocyanate and quaternized rosin ester chain extender is 1:(2.2-2.4):(1-1.2).
3. The method for preparing a bio-based thermoplastic polyurethane elastomer according to claim 2, characterized in that: The polyol is polytetramethylene ether diol, polybutylene adipate diol or polycaprolactone diol; the diisocyanate is 4,4'-methylenebis(phenyl isocyanate) or toluene-2,4-diisocyanate.
4. The method for preparing a bio-based thermoplastic polyurethane elastomer according to claim 2, characterized in that: The preparation method of the quaternized rosin acid ester chain extender is: Step (1), adding rosin acid, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and 4-dimethylaminopyridine to N,N-dimethylformamide, stirring and activating at room temperature for 20-40 minutes, then adding diethanolamine, stirring and reacting for 12-18 hours, transferring the solution to a separatory funnel, adding water and ethyl acetate, shaking and standing to separate, drying the organic layer with anhydrous sodium sulfate to remove water, and recrystallizing the filtrate to obtain a rosin acid ester intermediate; Step (2), adding a rosin acid ester intermediate, a bromohydrin compound and potassium carbonate to acetonitrile to carry out a substitution reaction, then adding a bromohydrin compound to carry out a quaternization reaction, distilling under reduced pressure, adding the product after washing with water to a mixed solution of ethanol and ethyl acetate, and recrystallizing to obtain a quaternized rosin acid ester chain extender.
5. The method for preparing a bio-based thermoplastic polyurethane elastomer according to claim 4, characterized in that: In the step (1), the molar ratio of rosin acid, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, 4-dimethylaminopyridine and diethanolamine is (2-2.2):(2.2-2.4):(0.14-0.18):
1.
6. The method for preparing a bio-based thermoplastic polyurethane elastomer according to claim 4, characterized in that: In the step (2), the molar ratio of the rosin acid ester intermediate, the bromohydrin compound and potassium carbonate is 1:(2-2.4):(2-2.2).
7. The method for preparing a bio-based thermoplastic polyurethane elastomer according to claim 6, characterized in that: The structural formula of the bromohydrin compound is , n is any integer from 2 to 8.
8. The method for preparing a bio-based thermoplastic polyurethane elastomer according to claim 4, characterized in that: In the step (2), the substitution reaction is carried out at 40-50° C. for 4-6 hours; and the quaternization reaction is carried out at 80-85° C. for 12-18 hours under condensation reflux.
Citation Information
Patent Citations
Bromine-containing room-temperature phosphorescent waterborne polyurethane and preparation method thereof
CN107987010A
Method of preparing quaternized esters of carboxylic acids and aminoalcohols
SU793998A1
Hydrophilic apertured formed film
US20110293886A1
Multifunctional polyol resins, curable compositions, and methods thereof
US20230303756A1
Reaction of rosin acid adducts with dialkanolamines
US2982750A