Preparation method of low-temperature-resistant polyether ester type polyurethane elastomer

By introducing carbonate and polyether coblock polymers into polyurethane materials and combining polyester segments, low-temperature resistant polyether ester polyurethane elastomers are prepared, which solves the performance problems of conventional polyurethane materials in low temperature environments and improves the performance of them. The hydrolysis resistance of the material is achieved, and the combination of high strength and environmental protection is achieved.

CN119081055APending Publication Date: 2024-12-06SHANDONG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411193361.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Conventional polyurethane materials are difficult to maintain good mechanical properties under low temperature environments, and the carbonate polyurethane synthesis process is complex and costly, which limits its application.

Method used

The low-temperature resistant polyether ester type polyurethane elastomer is synthesized by using carbonate and polyether coblock polymers. The mechanical properties of the material are regulated by introducing polyester segments, and the preparation method for specific raw material composition and process steps are prepared to improve the low-temperature resistance of the material. and hydrolysis resistance.

Benefits of technology

It has achieved the improvement of high strength, heat resistance, wear resistance and low temperature resistance of polyurethane materials, and has environmentally friendly properties, solving the problem of poor physical compatibility between polyester and polyether segments, and realizing controllable material structure design.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081055A_ABST
    Figure CN119081055A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a low-temperature-resistant polyether ester type polyurethane elastomer, and belongs to the technical field of polyurethane materials. The invention relates to an ultraviolet-resistant polyurethane coating which is prepared by mixing a component A and a component B, wherein the component A is prepared from the following raw materials in parts by mass: 20-70 parts of polymer polyol, 10-90 parts of polyester polyol, 0.08-0.12 part of a defoaming agent, 0.005-0.01 part of an antioxidant, 0.05-0.1 part of an ultraviolet light absorber and 12-40 parts of isocyanate; and the component B is prepared from the following raw materials in parts by mass: 11-20 parts of a small molecular chain extender. The low-temperature-resistant polyether ester type polyurethane elastomer disclosed by the invention has the advantages of high strength, high elasticity and high wear resistance brought by carbonate bonds and flexibility and low-temperature resistance brought by ether bonds, and can be widely applied to the aspects of coatings, adhesives, foams, high-performance elastomers and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyurethane materials, and specifically designs a method for preparing a low-temperature resistant polyether ester type polyurethane elastomer. Background Art

[0002] Polyurethane is widely used in many fields due to its many advantages such as high strength, high elasticity, and high wear resistance. However, conventional polyurethane materials are difficult to maintain good mechanical properties in low temperature environments, so it is of great significance to improve the low temperature resistance of polyurethane elastomers. Polycarbonate polyurethane has excellent mechanical properties, high heat resistance, excellent low-temperature toughness, and excellent hydrolysis resistance and aging resistance. However, the synthesis process of carbonate polyurethane is complicated and the cost is high, which limits its application in many fields. Carbonate and polyether block copolymers (PCEL) have high crystallinity and temperature resistance due to the carbonate bonds contained in their segment structures, and the flexibility and low temperature resistance brought by the ether bonds. The polyurethane materials synthesized with them as raw materials have broad application prospects.

[0003] The purpose of the present invention is to prepare a low-temperature resistant polyether ester type polyurethane elastomer, introduce carbonate and polyether co-block polymers to improve the low-temperature resistance and hydrolysis resistance of the polyurethane elastomer, and adjust the mechanical properties of the polyurethane material by introducing polyester segments during the synthesis process. The present invention also provides a preparation method thereof.

[0004] The low-temperature resistant polyetherester polyurethane elastomer of the present invention is prepared by mixing component A and component B, wherein component A is composed of the following raw materials in parts by weight: 20 to 70 parts of polymer polyol, 10 to 90 parts of polyester polyol, 0.08 to 0.12 parts of defoaming agent, 0.005 to 0.01 parts of antioxidant, 0.05 to 0.1 parts of ultraviolet light absorber, and 12 to 40 parts of isocyanate;

[0005] Component B is composed of the following raw materials in parts by weight: 11 to 20 parts of a small molecule chain extender.

[0006] in:

[0007] The mass ratio of component A to component B is 7 to 10:1;

[0008] The polymer polyol is a polycarbonate polyether polyol with a molecular weight of 1610, specifically PCE220D produced by Hefei Puli Advanced Materials Technology Co., Ltd., and its chemical structure diagram is as follows:

[0009]

[0010] The polyester polyol has a molecular weight of 2000 and includes one or more of polyethylene adipate glycol / butylene adipate glycol type diol (PEBL), polyethylene adipate glycol type diol (PEL), and polybutylene adipate glycol type diol (PBL).

[0011] The mass ratio of polyester polyol to polymer polyol is 1-9.

[0012] The isocyanate is one or more of toluene diisocyanate, diphenylmethane diisocyanate and hexamethylene diisocyanate.

[0013] The chain extender is 3,3'-dichloro-4,4'-diaminodiphenylmethane (MOCA) or 1,4-butanediol (BDO).

[0014] The antioxidant is 4-hydroxy 3,5-tert-butylphenyl propionic acid.

[0015] The ultraviolet absorber is 2-hydroxy-4-methoxybenzophenone.

[0016] The defoamer is a polysilicone oil defoamer, such as BYK-065.

[0017] The method for preparing a low-temperature resistant polyether ester type polyurethane elastomer of the present invention comprises the following steps:

[0018] (1) Heat the polymer polyol to 100-115°C, stir, and remove moisture in vacuum. Cool to 50°C, add to the measured isocyanate, maintain the temperature at 80-85°C for 2-3 hours, then add the measured polyester polyol to continue the reaction until the NCO% reaches the designed value, add the measured antioxidant, ultraviolet light absorber, and defoaming agent, stir and defoam, and obtain component A;

[0019] (2) Weighing a designed amount of a small molecule chain extender, melting it at 130-140° C. and adding it to component A, stirring it thoroughly and evenly, and after vacuum degassing, pouring it into a mold and pressing it into a test piece to obtain a low-temperature resistant polyetherester type polyurethane elastomer.

[0020] The beneficial effects of the present invention are as follows:

[0021] The present invention adopts polycarbonate polyether co-block polymer polyol to synthesize polyurethane material, which solves the problem of poor physical compatibility of polyester and polyether segments, and realizes the controllable design of polycarbonate-polyether-polyester segments in the material structure by being miscible with polyester polyol in any ratio. The elastomer structure contains polycarbonate and polyester rigid segments, which give the elastomer material high strength, excellent heat resistance and wear resistance, and the polyether segments give the elastomer material excellent low temperature resistance and hydrolysis resistance. In addition, the PCEL structure contains about 25-30% mass fraction of carbon dioxide, that is, each kilogram of PCEL product has a carbon neutrality benefit of 25-30%, which truly realizes the special significance of combining the excellent performance of polyurethane elastomers with ecological environmental protection. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is the infrared spectrum of the polyether ester polyurethane elastomer prepared in Example 1.

[0023] Figure 2 This is the DSC graph of the polyether ester polyurethane elastomer prepared in Example 1. DETAILED DESCRIPTION

[0024] The present invention is specifically described and illustrated below in conjunction with embodiments.

[0025] Example 1

[0026] The polyetherester polyurethane elastomer is prepared from component A and component B, and the mass ratio of component A to component B is 10:1;

[0027] Component A consists of the following raw materials in parts by weight:

[0028]

[0029] Component B is composed of the following raw materials in parts by weight:

[0030]

[0031] The preparation process of the low temperature resistant polyether ester type polyurethane elastomer is as follows:

[0032] (1) According to the composition of the above-mentioned low-temperature resistant polyether ester type polyurethane elastomer, weigh the corresponding mass fractions of the raw materials;

[0033] (2) PCE220D was heated to 115°C, stirred, and vacuum-dried to remove moisture. The temperature was lowered to 50°C, and then added to the measured amount of toluene diisocyanate, and the temperature was maintained at 85°C for reaction for 2 hours. Then the measured amount of PEBL was added to continue the reaction until the NCO% reached the designed value, and the measured amount of 4-hydroxy 3,5-tert-butylphenyl propionic acid, 2-hydroxy-4-methoxybenzophenone, and BYK-065 were added, and the mixture was stirred and degassed to obtain component A;

[0034] (3) 11.6 parts of MOCA were weighed, melted at 135° C., and added to component A. The mixture was thoroughly stirred and, after vacuum degassing, poured into a mold and pressed into a test piece to obtain a low-temperature resistant polyetherester polyurethane elastomer.

[0035] Example 2

[0036] The polyetherester type polyurethane elastomer is prepared from component A and component B, and the mass ratio of component A to component B is 9:1;

[0037] Component A consists of the following raw materials in parts by weight:

[0038]

[0039] Component B is composed of the following raw materials in parts by weight:

[0040] MOCA 13 copies

[0041] The preparation process of the low temperature resistant polyether ester type polyurethane elastomer is as follows:

[0042] (1) According to the composition of the above-mentioned low-temperature resistant polyether ester type polyurethane elastomer, weigh the corresponding mass fractions of the raw materials;

[0043] (2) PCE220D was heated to 115°C, stirred, and vacuum-dried to remove moisture. The temperature was lowered to 50°C, and then added to the measured toluene diisocyanate, and the temperature was maintained at 85°C for reaction for 2 hours. Then, the measured PEL was added to continue the reaction until the NCO% reached the designed value, and the measured 4-hydroxy 3,5-tert-butylphenyl propionic acid, 2-hydroxy-4-methoxybenzophenone, and BYK-065 were added, and the mixture was stirred for degassing to obtain component A;

[0044] (3) 13 parts of MOCA were weighed, melted at 135° C., and added to component A. The mixture was thoroughly stirred, and after vacuum degassing, the mixture was poured into a mold and pressed into a test piece to obtain a low-temperature resistant polyetherester polyurethane elastomer.

[0045] Example 3

[0046] The polyetherester polyurethane elastomer is prepared from component A and component B, and the mass ratio of component A to component B is 7:1;

[0047] Component A consists of the following raw materials in parts by weight:

[0048]

[0049] Component B is composed of the following raw materials in parts by weight:

[0050] BDO 12.4 parts

[0051] The preparation process of the low temperature resistant polyether ester type polyurethane elastomer is as follows:

[0052] (1) According to the composition of the above-mentioned low-temperature resistant polyether ester type polyurethane elastomer, weigh the corresponding mass fractions of the raw materials;

[0053] (2) Heat PCE220D to 115°C, stir, and remove moisture in vacuum. Cool to 50°C, then add measured hexamethylene diisocyanate, maintain the temperature at 85°C for 2h, then add measured PBL to continue the reaction until the NCO% reaches the designed value, add measured 4-hydroxy 3,5-tert-butylphenyl propionic acid, 2-hydroxy-4-methoxybenzophenone, BYK-065, stir and degas, and obtain component A;

[0054] (3) 12.4 parts of BDO were weighed, melted at 135° C., and added to component A. The mixture was thoroughly stirred and, after vacuum degassing, poured into a mold and pressed into a test piece to obtain a low-temperature resistant polyetherester polyurethane elastomer.

[0055] Example 4

[0056] The polyetherester polyurethane elastomer is prepared from component A and component B, and the mass ratio of component A to component B is 9.5:1;

[0057] Component A consists of the following raw materials in parts by weight:

[0058]

[0059] Component B is composed of the following raw materials in parts by weight:

[0060] MOCA 13 copies

[0061] The preparation process of the low temperature resistant polyether ester type polyurethane elastomer is as follows:

[0062] (1) According to the composition of the above-mentioned low-temperature resistant polyether ester type polyurethane elastomer, weigh the corresponding mass fractions of the raw materials;

[0063] (2) PCE220D was heated to 115°C, stirred, and vacuum-dried to remove moisture. The temperature was lowered to 50°C, and then added to the measured toluene diisocyanate, and the temperature was maintained at 85°C for 2 hours, until the NCO% reached the designed value, and the measured 4-hydroxy 3,5-tert-butylphenyl propionic acid, 2-hydroxy-4-methoxybenzophenone, and BYK-065 were added, and the mixture was stirred and degassed to obtain component A;

[0064] (3) 13 parts of MOCA were weighed, melted at 135° C., and added to component A. The mixture was thoroughly stirred, and after vacuum degassing, the mixture was poured into a mold and pressed into a test piece to obtain a low-temperature resistant polyetherester polyurethane elastomer.

[0065] Compared with Example 1, Comparative Example 1 uses polyester polyol to synthesize the prepolymer.

[0066] The polyester polyurethane elastomer is prepared from component A and component B, and the mass ratio of component A to component B is 7:1;

[0067] Component A consists of the following raw materials in parts by weight:

[0068]

[0069] Component B is composed of the following raw materials in parts by weight:

[0070] BDO 13 copies

[0071] The preparation process of the low temperature resistant polyether ester type polyurethane elastomer is as follows:

[0072] (1) According to the composition of the above-mentioned low-temperature resistant polyether ester type polyurethane elastomer, weigh the corresponding mass fractions of the raw materials;

[0073] (2) PEBL was heated to 115°C, stirred, and vacuum-dried to remove moisture. The temperature was lowered to 50°C, and then added to the measured amount of diphenylmethane diisocyanate, and the temperature was maintained at 85°C for 2 hours, until the NCO% reached the designed value, and the measured amount of 4-hydroxy 3,5-tert-butylphenyl propionic acid, 2-hydroxy-4-methoxybenzophenone, and BYK-065 were added, and stirred to degas, to obtain component A;

[0074] (3) 13 parts of BDO were weighed, melted at 135° C. and added to component A, and the mixture was thoroughly stirred. After vacuum degassing, the mixture was poured into a mold and pressed into a test piece to obtain a low-temperature resistant polyetherester polyurethane elastomer.

[0075] Table 1 Performance parameters of polyether ester polyurethane elastomers in Examples 1 to 4 and Comparative Examples 1 to 2

[0076]

[0077] In summary, the low-temperature resistant polyetherester polyurethane elastomer described in the present invention has good tensile properties and has better hydrolysis resistance and low-temperature resistance than conventional polyester polyurethane elastomers.

Claims

1. A method for preparing a low-temperature resistant polyetherester polyurethane elastomer, characterized in that: The method is prepared by mixing component A and component B, wherein component A is composed of the following raw materials in parts by weight: 20 to 70 parts of polymer polyol, 10 to 90 parts of polyester polyol, 0.08 to 0.12 parts of defoamer, 0.005 to 0.01 parts of antioxidant, 0.05 to 0.1 parts of ultraviolet light absorber, and 12 to 40 parts of isocyanate; Component B is composed of the following raw materials in parts by weight: 11 to 20 parts of a small molecule chain extender.

2. The low-temperature resistant polyetherester polyurethane elastomer according to claim 1, characterized in that: The mass ratio of component A to component B is 7 to 10:

1.

3. The polymer polyol according to claim 1 is a polycarbonate polyether polyol with a molecular weight of 1610, specifically PCE220D produced by Hefei Puli Advanced Materials Technology Co., Ltd., and its chemical structure diagram is as follows:

4. The polyester polyol according to claim 1 has a molecular weight of 2000, and comprises one or more of polyethylene adipate / butylene adipate diol (PEBL), polyethylene adipate diol (PEL), and polybutylene adipate diol (PBL).

5. The low-temperature resistant polyetherester polyurethane elastomer according to claim 1, characterized in that: The mass fraction ratio of polymer polyol to polyester polyol is 1-9.

6. The low-temperature resistant polyetherester polyurethane elastomer according to claim 1, characterized in that: The isocyanate is one or more of toluene diisocyanate, diphenylmethane diisocyanate and hexamethylene diisocyanate.

7. The low-temperature resistant polyetherester polyurethane elastomer according to claim 1, characterized in that: The small molecule chain extender is 3,3'-dichloro-4,4'-diaminodiphenylmethane (MOCA) or 1,4-butanediol (BDO).

8. The low-temperature resistant polyetherester polyurethane elastomer according to claim 1, characterized in that: The antioxidant is 4-hydroxy 3,5-tert-butylphenylpropionic acid.

9. The low-temperature resistant polyetherester polyurethane elastomer according to claim 1, characterized in that: The ultraviolet absorber is 2-hydroxy-4-methoxybenzophenone.

10. The low-temperature resistant polyetherester polyurethane elastomer according to claim 1, characterized in that: The defoaming agent is a polysilicone oil defoaming agent, such as BYK-065.

11. A method for preparing a low-temperature resistant polyether ester type polyurethane elastomer according to any one of claims 1 to 10, characterized in that The following steps are involved: (1) Heat the polymer polyol to 100-115°C, stir, and remove moisture in vacuum. Cool to 50°C, add to the measured isocyanate, maintain the temperature at 80-85°C for 2-3 hours, then add the measured polyester polyol to continue the reaction until the NCO% reaches the designed value, add the measured antioxidant, ultraviolet light absorber, and defoaming agent, stir and defoam, and obtain component A; (2) Weighing a designed amount of a small molecule chain extender, melting it at 130-140° C. and adding it to component A, stirring it thoroughly and evenly, and after vacuum degassing, pouring it into a mold and pressing it into a test piece to obtain a low-temperature resistant polyetherester type polyurethane elastomer.