Electrochromic polymer, electrochromic film as well as preparation method and application of electrochromic polymer and electrochromic film
By polymerizing the first thiophene derivative of cyclopentylmethoxy and bromine with the second thiophene derivative of polyphenylene ring polythiophene ring, the problem of insufficient stability of existing electrochromic materials is solved, and a low driving potential is achieved , electrochromic behavior with fast response rate and high coloring efficiency, and electrochromic polymer films have excellent stability.
Patent Information
- Application Number
- CN202411185859.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-27
AI Technical Summary
Existing electrochromic materials that can achieve red, purple to transparent transformations are insufficient in stability, and the response rate and coloring efficiency are not high.
The first thiophene derivative containing cyclopentylmethoxy and bromine is polymerized with a second thiophene derivative containing a plurality of benzene rings and a plurality of thiophene rings in the molecule to adjust the band gap of the polymer to achieve color and transparent color. The electrochromic polymer was prepared by polymerization and purification treatment.
The electrochromic behavior of low driving potential, fast response rate, high coloring efficiency and good stability in the color change process is achieved, and the electrochromic polymer film has excellent electrochemical stability, thermal stability and cyclic stability.
Smart Images

Figure CN119081073A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrochromic materials, and in particular to an electrochromic polymer, an electrochromic film, and a preparation method and application thereof. Background Art
[0002] Electrochromic materials refer to materials whose optical properties change due to the charge transfer process under the action of an external electric field. They have broad application prospects in the fields of flexible displays, smart windows, anti-glare rearview mirrors, and military intelligent camouflage. Electrochromic materials include transition metal oxides, violaceous small molecules, conductive polymers, etc. Among them, conductive polymers have become a hot spot in the current research and application of electrochromic due to their advantages such as designable structure, rich color changes, high contrast, fast response rate, high coloring efficiency and good stability. The development of new conductive polymers with excellent electrochromic properties, especially red and purple, is of great significance to the research on polymer electrochromism. However, the existing electrochromic materials that can achieve red and purple to transparent transformation still have the problem of insufficient stability. Summary of the invention
[0003] In view of one or more technical problems existing in the prior art, the present invention provides an electrochromic polymer, an electrochromic film, and a preparation method and application thereof. The electrochromic polymer provided by the present invention exhibits obvious electrochromic behavior and can achieve reversible changes between colored and transparent colors. The color change process has a low driving potential, a fast response rate, a high coloring efficiency, and good stability.
[0004] The present invention provides an electrochromic polymer, which is obtained by polymerizing a first thiophene derivative and a second thiophene derivative; the structural formula of the first thiophene derivative is as shown in formula (1): The second thiophene derivative is a thiophene derivative including a plurality of benzene rings and a plurality of thiophene rings.
[0005] Preferably, the second thiophene derivative is selected from one or more of formulas (2)-(3);
[0006]
[0007] Preferably, the structural formula of the electrochromic polymer is one of formulas (4)-(5);
[0008]
[0009] Wherein n is 8 to 100.
[0010] In a second aspect, the present invention provides a method for preparing the electrochromic polymer according to the first aspect, the preparation method comprising:
[0011] The first thiophene derivative, the second thiophene derivative, a solvent, potassium carbonate, palladium acetate and pivalic acid are mixed, and subjected to polymerization reaction and a first purification treatment to obtain an electrochromic polymer.
[0012] Preferably, the molar ratio of the first thiophene derivative to potassium carbonate is 1:2-4;
[0013] The molar ratio of the first thiophene derivative to palladium acetate is 1:0.02-0.2;
[0014] The molar ratio of the first thiophene derivative to pivalic acid is 1:0.1-0.25; and / or
[0015] The usage ratio of the first thiophene derivative to the solvent is 1 mmol:100-500 mL. Preferably, the solvent is a non-protonic polar solvent.
[0016] Preferably, the polymerization reaction temperature is 100-120°C and the time is 48-96h; and / or
[0017] The first purification treatment includes: mixing the reaction solution after the polymerization reaction with methanol, extracting the precipitate with methanol, n-hexane and chloroform in sequence, concentrating the solution after chloroform extraction, mixing it with methanol again, filtering and drying.
[0018] Preferably, the preparation method of the first thiophene derivative comprises: (i) subjecting 3,4-dimethoxythiophene and cyclopentylmethanol to a heating reflux reaction in the presence of a catalyst, and a second purification treatment to obtain an intermediate product; preferably, the catalyst is p-toluenesulfonic acid monohydrate; (ii) subjecting the intermediate product to a bromination reaction with N-bromosuccinimide, and subjecting the intermediate product to a third purification treatment to obtain the first thiophene derivative.
[0019] Preferably, the second purification treatment comprises: separating the reaction solution after the heating reflux reaction to obtain a first aqueous phase and a first organic phase, then extracting the first aqueous phase, combining the obtained second organic phase with the first organic phase, and then drying and wet-loading the obtained phase on a silica gel column; and / or
[0020] The third purification treatment includes: separating the reaction liquid after the bromination reaction to obtain a second aqueous phase and a third organic phase, then extracting the second aqueous phase, and combining the obtained fourth organic phase with the third organic phase, and then drying and dry-loading the mixture through a silica gel column.
[0021] The present invention provides an electrochromic polymer film in a third aspect, which is made from the electrochromic polymer described in the first aspect; preferably, the electrochromic polymer film has a thickness of 200 to 800 nm.
[0022] In a fourth aspect, the present invention provides an application of the electrochromic polymer film described in the third aspect, which is applied to an electrochromic device.
[0023] Compared with the prior art, the present invention has at least the following beneficial effects:
[0024] The present invention uses a first thiophene derivative containing cyclopentylmethoxy and bromine and a second thiophene derivative containing multiple benzene rings and multiple thiophene rings in the molecule for polymerization, introduces the structural unit of the second thiophene derivative into the main chain of the first thiophene derivative, and uses its different planar characteristics to adjust the band gap of the polymer, so that the electrochromic polymer exhibits obvious electrochromic behavior, can achieve reversible changes between colored and transparent colors, and the color change process has low driving potential, fast response rate, high coloring efficiency and good stability. The electrochromic polymer film prepared by the electrochromic polymer of the present invention has excellent electrochemical stability, thermal stability and cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0026] Figure 1 It is the nuclear magnetic hydrogen spectrum of the intermediate product in the preparation process of the first thiophene derivative provided by the present invention;
[0027] Figure 2 is the nuclear magnetic hydrogen spectrum of the first thiophene derivative provided by the present invention;
[0028] Figure 3 is the H NMR spectrum of the electrochromic polymer provided in Example 1 of the present invention;
[0029] Figure 4 is the H NMR spectrum of the electrochromic polymer provided in Example 2 of the present invention;
[0030] Figure 5 It is a spectral absorption curve and color comparison diagram of the electrochromic polymer solution provided in Examples 1-2 of the present invention;
[0031] Figure 6 is the thermal stability curve of the electrochromic polymer provided in Examples 1-2 of the present invention;
[0032] Figure 7 is a comparison diagram of the ultraviolet-visible absorption spectra and color changes of the electrochromic polymer film provided in Example 3 of the present invention at different potentials;
[0033] Figure 8 is a comparison diagram of the ultraviolet-visible absorption spectra and color changes of the electrochromic polymer film provided in Example 4 of the present invention at different potentials;
[0034] Fig. 9 is the cyclic voltammetry curve of the electrochromic polymer film provided in Example 3 of the present invention at different scanning rates;
[0035] Fig.10 is the cyclic voltammetry curve of the electrochromic polymer film provided by Example 4 of the present invention at different scanning rates;
[0036] Fig.11 The timing transmittance response and stability curve of the electrochromic polymer film provided in Example 3 of the present invention;
[0037] Fig.12 This is the timing transmittance response and stability curve of the electrochromic polymer film provided in Example 4 of the present invention. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0039] The present invention provides an electrochromic polymer, which is obtained by polymerizing a first thiophene derivative and a second thiophene derivative; the structural formula of the first thiophene derivative is as shown in formula (1): The second thiophene derivative is a thiophene derivative including a plurality of benzene rings and a plurality of thiophene rings.
[0040] The present invention uses a first thiophene derivative containing cyclopentylmethoxy and bromine and a second thiophene derivative containing multiple benzene rings and multiple thiophene rings in the molecule for polymerization, introduces the structural unit of the second thiophene derivative into the main chain of the first thiophene derivative, and uses its different planar characteristics to adjust the band gap of the polymer, so that the electrochromic polymer exhibits obvious electrochromic behavior, can achieve reversible changes between colored and transparent colors, and the color change process has low driving potential, fast response rate, high coloring efficiency and good stability. The electrochromic polymer film prepared by the electrochromic polymer of the present invention has excellent electrochemical stability, thermal stability and cycle stability.
[0041] According to some preferred embodiments, the second thiophene derivative is selected from one or more of formulas (2)-(3);
[0042]
[0043] According to some preferred embodiments, the electrochromic polymer has a structural formula of one of formulas (4)-(5);
[0044] Wherein n is 8 to 100.
[0045] In the second thiophene derivative having the structure of the above formula (2), sp 3 The availability of hybridized carbon atoms allows functional side chains to be easily attached to its structural unit to increase its solubility in organic solvents. In addition, the inherent coplanar "ladder" structure of its structural unit enhances the degree of π electron delocalization, making it highly electron-rich. Copolymerization with the first thiophene derivative having the structure of the above formula (1) can obtain an electrochromic polymer having the structure of the above formula (4), which can achieve reversible electrochromic behavior between red and transparent colors.
[0046] Compared with the second thiophene derivative having the structure of the above formula (2), the second thiophene derivative having the structure of the above formula (3) has better planarity and regularity while maintaining a good conjugated structure. When cycloalkoxythiophene is copolymerized with the second thiophene derivative having the structure of the above formula (3), it has a lower band gap, so that the absorption spectrum of the polymer is red-shifted to show purple, and the electrochromic polymer having the structure of the above formula (5) copolymerized with the first thiophene derivative having the structure of the above formula (1) can achieve reversible electrochromic behavior between purple and transparent colors.
[0047] In a second aspect, the present invention provides a method for preparing the electrochromic polymer according to the first aspect, the preparation method comprising:
[0048] The first thiophene derivative, the second thiophene derivative, a solvent, potassium carbonate, palladium acetate and pivalic acid are mixed, and subjected to polymerization reaction and a first purification treatment to obtain an electrochromic polymer.
[0049] According to some preferred embodiments, the molar ratio of the first thiophene derivative to potassium carbonate is 1:2-4;
[0050] The molar ratio of the first thiophene derivative to palladium acetate is 1:0.02-0.2;
[0051] The molar ratio of the first thiophene derivative to pivalic acid is 1:0.1-0.25; and / or
[0052] The usage ratio of the first thiophene derivative to the solvent is 1 mmol:100-500 mL. Preferably, the solvent is a non-protonic polar solvent.
[0053] According to some preferred embodiments, the polymerization reaction temperature is 100-120° C. and the time is 48-96 hours. The polymerization reaction of the present invention is an arylation coupling polymerization reaction, which is carried out under a protective atmosphere.
[0054] According to some preferred embodiments, the first purification treatment comprises: mixing the reaction solution after the polymerization reaction with methanol, extracting the precipitate with methanol, n-hexane and chloroform in sequence, concentrating the solution after chloroform extraction and mixing it with methanol again, filtering and drying.
[0055] According to some preferred embodiments, the preparation method of the first thiophene derivative comprises: (i) subjecting 3,4-dimethoxythiophene and cyclopentylmethanol to a heating reflux reaction under the action of a catalyst, and a second purification treatment to obtain an intermediate product; preferably, the catalyst is p-toluenesulfonic acid-hydrate; (ii) subjecting the intermediate product to a bromination reaction with N-bromosuccinimide, and a third purification treatment to obtain the first thiophene derivative. It should be noted that in the preparation process of the first thiophene derivative, in addition to the above-mentioned raw materials, a solvent for dissolving and dispersing the reactants is also included.
[0056] According to some preferred embodiments, the second purification treatment includes: separating the reaction liquid after the heating reflux reaction to obtain a first aqueous phase and a first organic phase, then extracting the first aqueous phase, and combining the obtained second organic phase with the first organic phase, and then drying and wet-loading the mixture through a silica gel column.
[0057] According to some preferred embodiments, the third purification treatment includes: separating the reaction liquid after the bromination reaction to obtain a second aqueous phase and a third organic phase, then extracting the second aqueous phase, and combining the obtained fourth organic phase with the third organic phase, and then drying and dry-loading it on a silica gel column.
[0058] In some preferred embodiments of the present invention, during the second purification treatment and the third purification treatment, the solvent used for extraction is dichloromethane.
[0059] In some preferred embodiments of the present invention, during the second purification treatment and the third purification treatment, the desiccant used for drying is anhydrous magnesium sulfate.
[0060] In some preferred embodiments of the present invention, in the second purification process, the eluent used in the wet loading of the sample through the silica gel column is a mixture of petroleum ether and dichloromethane.
[0061] In some preferred embodiments of the present invention, in the third purification process, the eluent used for dry loading on the silica gel column is a mixture of petroleum ether and dichloromethane.
[0062] The present invention provides an electrochromic polymer film in a third aspect, which is prepared by using the electrochromic polymer described in the first aspect.
[0063] The polymer provided by the invention is soluble in organic solvents such as chloroform, tetrahydrofuran, toluene, etc., and a layer of electrochromic polymer film can be formed on the surface of the conductive material by spraying or scraping.
[0064] According to some preferred embodiments, the thickness of the electrochromic polymer film is 200-800 nm.
[0065] In a fourth aspect, the present invention provides an application of the electrochromic polymer film described in the third aspect, which is applied to an electrochromic device.
[0066] In order to more clearly illustrate the technical solutions and advantages of the present invention, the present invention is further described below in conjunction with the examples. The present invention does not specifically limit the sources of the reagents used in the examples and comparative examples, and the reagents can be directly purchased or synthesized by themselves.
[0067] Example 1
[0068] Preparation of the first thiophene derivative:
[0069] (i) 0.1 mol of 3,4-dimethoxythiophene, 0.25 mol of cyclopentylmethanol and 0.001 mol of p-toluenesulfonic acid monohydrate were dissolved in 200 mL of toluene and placed in a 500 mL single-necked flask, connected to a Soxhlet extractor with a molecular sieve and a condenser, refluxed and stirred for reaction for 24 h, then cooled to room temperature, poured the reaction solution into water, separated and collected the organic phase, the aqueous phase was extracted twice with 20 mL of dichloromethane, the organic phases were combined, dried over anhydrous magnesium sulfate, and wet-loaded on a silica gel column, the eluent being a mixture of petroleum ether and dichloromethane in a volume ratio of 4:1, to obtain a white solid, recorded as an intermediate product, with a yield of 46%; the nuclear magnetic hydrogen spectrum of the intermediate product 1H NMR (400 MHz, Chloroform-d) is as follows Figure 1 , it can be seen that δ6.16(s,1H), δ3.85(s,2H), δ2.40(s,1H), δ1.59(s,8H), proving that the intermediate product with the molecular structure in the following reaction formula was obtained.
[0070]
[0071] (ii) 0.1 mmol of white solid (intermediate product) was dissolved in 20 mL of chloroform and placed in a 100 mL two-necked flask. The two-necked flask was protected by argon and covered with tin foil to avoid light. 0.3 mmol of NBS (N-bromosuccinimide) was dissolved in 10 mL of N,N-dimethylformamide (DMF) and slowly injected into the two-necked flask through a syringe. The reaction was stirred for 36 hours. The reaction solution was poured into water, and the organic phase was collected by separation. The aqueous phase was extracted twice with 20 mL of dichloromethane. The organic phases were combined and dried over anhydrous magnesium sulfate. The sample was passed through a silica gel column by dry method. The eluent was a mixture of petroleum ether and dichloromethane in a volume ratio of 4:1 to obtain a colorless oily liquid, which was recorded as the first thiophene derivative. The yield was 80%. The nuclear magnetic hydrogen spectrum of the first thiophene derivative 1H NMR (400 MHz, Chloroform-d) is as follows Figure 2 It can be seen that δ3.92 (s, 2H), δ2.31 (s, 1H), δ1.90-1.30 (m, 8H), which proves that the first thiophene derivative with the molecular structure in the following reaction formula was obtained.
[0072]
[0073] Preparation of electrochromic polymers:
[0074] 0.1mmol of the first thiophene derivative, 0.1mmol of the second thiophene derivative (4,9-dihydro-s-benzoindene[1,2-b:5,6-b']dithiophene), 0.002mmol of palladium acetate, 0.3mmol of potassium carbonate and 0.025mmol of pivalic acid were placed in a 25mL two-necked bottle, ventilated and injected with nitrogen, and 10mL of anhydrous N,N-dimethylacetamide (DMAC) was injected, and then ventilated and filled with nitrogen, heated to 120℃ and refluxed for reaction for 72h, cooled to room temperature after the reaction was completed, and the reaction solution was dripped into cold methanol for precipitation, and the precipitate was filtered and dried; then Soxhlet extraction was performed with methanol, n-hexane and chloroform respectively, and the extraction time for each time was 24h, the chloroform extract was concentrated to 15mL, and then dripped into cold methanol for precipitation to obtain a red solid, which was filtered and dried to obtain an electrochromic polymer, denoted as P1, with a yield of 56%. The nuclear magnetic hydrogen spectrum of the electrochromic polymer is as follows Figure 3 , proving that an electrochromic polymer with the molecular structure in the following reaction formula was prepared.
[0075]
[0076] Example 2
[0077] Preparation of the first thiophene derivative: same as Example 1.
[0078] Preparation of electrochromic polymer: 0.1mmol of the first thiophene derivative, 0.1mmol of the second thiophene derivative (tri(thieno[3,2-b]thiophene), 0.002mmol of palladium acetate, 0.3mmol of potassium carbonate and 0.025mmol of pivalic acid were placed in a 25mL two-necked bottle, ventilated and injected with nitrogen, 10mL of anhydrous N,N-dimethylacetamide (DMAC) was injected, ventilated and filled with nitrogen, heated to 120°C and refluxed for 72h, cooled to room temperature after the reaction, and the reaction solution was dripped into cold methanol for precipitation, and the precipitate was filtered and dried; then Soxhlet extraction was performed with methanol, n-hexane and chloroform, respectively, each extraction time was 24h, the chloroform extract was concentrated to 15mL, and then dripped into cold methanol to precipitate to obtain a purple solid, which was filtered and dried to obtain the target polymer P2, with a yield of 50%. The nuclear magnetic hydrogen spectrum of the electrochromic polymer is as follows Figure 4 , proving that an electrochromic polymer with the molecular structure in the following reaction formula was prepared.
[0079]
[0080] The electrochromic polymers prepared in Example 1 and Example 2 were dissolved in chloroform to prepare a concentration of 2×10 -4 mg / mL solution, measure the absorption curve and color of the solution ( Figure 5 , the horizontal axis is the wavelength, and the vertical axis is the absorbance). The electrochromic polymer P1 solution appears red, and the absorption peaks corresponding to the solution are at 521 nm when tested by a UV-visible spectrophotometer; the electrochromic polymer P2 solution appears purple, and the absorption peaks corresponding to the solution are at 559 nm when tested by a UV-visible spectrophotometer.
[0081] The present invention tests the thermal stability of the electrochromic polymers prepared in Example 1 and Example 2 ( Figure 6 , in the figure, the horizontal axis is temperature and the vertical axis is mass fraction). The thermal decomposition temperature of the two electrochromic polymers is greater than 300°C, indicating that they can be used in working environments with higher temperatures.
[0082] Example 3
[0083] An electrochromic polymer film is prepared by using the electrochromic polymer P1 prepared in Example 1; the preparation method of the electrochromic polymer film comprises:
[0084] The electrochromic polymer P1 was dissolved in chloroform to prepare a 4 mg / mL solution, and the insoluble matter was filtered out through a filter. The solution was then placed in a spray gun, the air pressure was controlled to be 2 MPa, and sprayed on a conductive glass. After spraying, the solution was placed in a vacuum drying oven at 40°C for vacuum drying to obtain an electrochromic polymer film (absorbance is 1.0).
[0085] Example 4
[0086] An electrochromic polymer film is prepared by using the electrochromic polymer P2 prepared in Example 2; the preparation method of the electrochromic polymer film comprises:
[0087] The electrochromic polymer P2 was dissolved in chloroform to prepare a 4 mg / mL solution, the insoluble matter was filtered out through a filter, and then placed in a spray gun, the air pressure was controlled to be 2 MPa, and sprayed on a conductive glass. After spraying, it was placed in a vacuum drying oven at 40°C for vacuum drying to obtain an electrochromic polymer film (absorbance is 1.0).
[0088] The present invention tests the spectral electrochemical performance of the electrochromic polymer films prepared in Example 3 and Example 4 at different voltages, using a three-electrode system, with a platinum wire as a counter electrode, a calibrated silver wire as a reference electrode, a polymer film as a working electrode, and a supporting electrolyte of 0.1 mol / L lithium perchlorate propylene carbonate solution. The spectral electrochemical spectra and coloration photos of the two electrochromic polymer films at different applied voltages ( Figure 7-8 , the horizontal axis is wavelength, the vertical axis is absorbance) It can be seen that both electrochromic polymer films have obvious electrochromic properties, and can achieve reversible changes from purple to transparent color at a relatively low voltage. Due to the accumulation of π-π* bonds, the obtained electrochromic polymer film has a certain red shift relative to the spectrum of the corresponding solution. The absorption peak of the film prepared by using electrochromic polymer P1 in Example 3 is 524nm ( Figure 7 ), a reversible change from red to transparent can be achieved at a lower voltage. Example 4 The absorption peak of the film made of electrochromic polymer P2 is 560nm ( Figure 8 ), a reversible change from colored to transparent can be achieved at a relatively low voltage.
[0089] The present invention also uses cyclic voltammetry to test the electrochromic polymer films prepared in Example 3 and Example 4. The cyclic voltammetry curves at different scanning rates characterize the electrochemical stability of the two electrochromic polymers ( Figure 9-10 , the horizontal axis is voltage, and the vertical axis is current density). The peak current density of the anode and cathode of the two electrochromic polymers gradually increases with the increase of scanning speed, and both have lower oxidation potentials. Among them, the initial oxidation potential of the electrochromic polymer P1 is 0.95V ( Fig. 9 ). The initial oxidation potential of the electrochromic polymer P2 is 0.7 V ( Fig.10 ), and the stability remains after multiple cyclic voltammetry scans.
[0090] The present invention uses a UV-visible spectrophotometer and an electrochemical workstation in combination, connects a three-electrode system to the electrochemical workstation, and places a quartz cuvette in the UV-visible spectrophotometer. While applying voltage to the electrochromic polymer film, the transmittance change at the wavelength of maximum transmittance is measured synchronously to test the cyclic stability of the two polymers. The transmittance of the electrochromic polymer P1 at 520nm still maintains a contrast ratio of 40% after 300 cycles ( Fig.11 The horizontal axis is time and the vertical axis is transmittance. The transmittance of the electrochromic polymer P2 at 560nm still maintains a contrast ratio of 49.1% after 600 cycles of switching. Fig.12 , where the horizontal axis is time and the vertical axis is transmittance), indicating that both polymers have a long cycle life.
[0091] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. An electrochromic polymer, It is characterized in that The electrochromic polymer is obtained by polymerizing a first thiophene derivative and a second thiophene derivative; the structural formula of the first thiophene derivative is as shown in formula (1): The second thiophene derivative is a thiophene derivative including a plurality of benzene rings and a plurality of thiophene rings.
2. The electrochromic polymer according to claim 1, It is characterized in that The second thiophene derivative is selected from one or more of formulas (2)-(3); 3. The electrochromic polymer according to claim 2, It is characterized in that The electrochromic polymer has a structural formula of one of formulas (4)-(5); Wherein n is 8 to 100.
4. A method for preparing the electrochromic polymer according to any one of claims 1 to 3, It is characterized in that The preparation method comprises: The first thiophene derivative, the second thiophene derivative, a solvent, potassium carbonate, palladium acetate and pivalic acid are mixed, and subjected to polymerization reaction and a first purification treatment to obtain an electrochromic polymer.
5. The preparation method according to claim 4, It is characterized in that The molar ratio of the first thiophene derivative to potassium carbonate is 1:2-4; The molar ratio of the first thiophene derivative to palladium acetate is 1:0.02-0.2; The molar ratio of the first thiophene derivative to pivalic acid is 1:0.1-0.25; and / or The usage ratio of the first thiophene derivative to the solvent is 1 mmol:100-500 mL. Preferably, the solvent is a non-protonic polar solvent.
6. The preparation method according to claim 4, It is characterized in that The polymerization reaction temperature is 100-120° C. and the reaction time is 48-96 hours; and / or The first purification treatment includes: mixing the reaction solution after the polymerization reaction with methanol, extracting the precipitate with methanol, n-hexane and chloroform in sequence, concentrating the solution after chloroform extraction, mixing it with methanol again, filtering and drying.
7. The preparation method according to claim 4, It is characterized in that The preparation method of the first thiophene derivative comprises: (i) subjecting 3,4-dimethoxythiophene and cyclopentylmethanol to a heating reflux reaction under the action of a catalyst, and a second purification treatment to obtain an intermediate product; preferably, the catalyst is p-toluenesulfonic acid monohydrate; (ii) subjecting the intermediate product to a bromination reaction with N-bromosuccinimide, and subjecting the intermediate product to a third purification treatment to obtain the first thiophene derivative.
8. The preparation method according to claim 7, It is characterized in that The second purification treatment comprises: separating the reaction liquid after the heating reflux reaction to obtain a first aqueous phase and a first organic phase, then extracting the first aqueous phase, combining the obtained second organic phase with the first organic phase, and then drying and wet-loading the obtained phase on a silica gel column; and / or The third purification treatment includes: separating the reaction liquid after the bromination reaction to obtain a second aqueous phase and a third organic phase, then extracting the second aqueous phase, and combining the obtained fourth organic phase with the third organic phase, and then drying and dry-loading the mixture through a silica gel column.
9. An electrochromic polymer film, It is characterized in that It is made from the electrochromic polymer according to any one of claims 1 to 3; preferably, the thickness of the electrochromic polymer film is 200 to 800 nm.
10. Use of the electrochromic polymer film according to claim 9, It is characterized in that Applied to electrochromic devices.
Citation Information
Patent Citations
Electrochromic polymer, preparation method thereof and electrochromic film
CN114605620A
Blue-to-transparent electrochromic polymer as well as preparation method and application thereof
CN115636924A
Condensed ring thiophene type purple to transparent electrochromic polymer as well as preparation method and application thereof
CN115636926A