Recyclable liquefied lignin-like composite material and preparation method thereof

Liquefied lignin is generated by reacting sodium sulfonate with quaternary ammonium salt and mixed with cellulose, which solves the problem of insufficient dispersion and interface compatibility of lignin materials, improves its processing performance and industrial application prospects, and avoids the Environmental pollution.

CN119081149APending Publication Date: 2024-12-06WUHAN TEXTILE UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411438710.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-15
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Due to poor dispersion and low interfacial compatibility, the prepared composite materials have many defects, which limit their application.

Method used

Sodium sulfonate reacts with quaternary ammonium salt in aqueous solvent, and drys at high temperature to obtain liquefied lignin, which is mixed with cellulose and sodium lignin sulfonate to form a soft solid of lignin to improve the dispersion of the material. Sex and interface compatibility.

Benefits of technology

It improves the dispersion and interface compatibility of lignin materials, enhances its processing performance, has a wide range of industrial application prospects, and avoids environmental hazards without the need for special solvents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005085787700000081
    Figure BDA0005085787700000081
  • Figure BDA0005085787700000101
    Figure BDA0005085787700000101
  • Figure HDA0005085787710000011
    Figure HDA0005085787710000011
Patent Text Reader

Abstract

The invention belongs to the field of high-performance materials, and particularly relates to quasi-liquefied lignin, a lignin composite material and a preparation method thereof.The preparation method of the quasi-liquefied lignin comprises the steps that sulfonated modified lignin and quaternary ammonium salt are dissolved in water respectively, and a sulfonated modified lignin solution and a quaternary ammonium salt solution are obtained after stirring is conducted for a certain time; mixing the obtained sulfonated modified lignin solution with a quaternary ammonium salt solution, stirring for a certain time, drying a reactant, taking a viscous liquid on the upper layer of the reactant, namely liquefied lignin, and preparing a lignin composite material based on the prepared liquefied lignin; the quasi-liquefied lignin obtained by the preparation method provided by the invention can overcome the problems of dispersion and interface of lignin, and meanwhile, the quasi-liquefied lignin promotes close contact and adhesion among the components when a composite material is prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of functional materials, in particular to the field of high-performance materials, and specifically to a recyclable composite material based on liquefied lignin. Background Art

[0002] Lignin is a natural high molecular compound that exists in large quantities in nature and is mainly used in the papermaking industry. Lignin is relatively easy to obtain because of its high carbon content and numerous active functional groups in its molecular structure, so it has the potential to prepare high-value products; however, the molecular structure, molecular weight, and properties of lignin obtained from natural plants rely on complex separation and testing, which leads to many difficulties in actual research.

[0003] Lignin itself has poor dispersibility and low interface compatibility as a basic material, which leads to many defects in the composite materials prepared therefrom and limits their application. The present invention uses lignin as a basic material, modifies lignin, prepares a lignin-like material, improves the dispersibility and interface compatibility of traditional lignin materials, and expects that the material can have stronger processing performance and prepare a composite material with multiple properties. Summary of the invention

[0004] In view of the many defects in the application of lignin materials in the prior art, the present invention intends to provide a liquefied lignin material based on lignin. The liquefied wood material has good dispersibility and interface compatibility and can be used in the production of industrial materials.

[0005] Furthermore, the concept of the present invention is to use sodium lignin sulfonate as a raw material, water as a solvent, and fully react with a quaternary ammonium salt, and the product after the reaction is dried at high temperature to obtain a quasi-liquefied layer to obtain quasi-liquefied lignin;

[0006] The quasi-liquefied lignin prepared by the present invention is a physical state of lignin material in the absence of solvent. The concept of the present invention is to modify the surface of sodium lignin sulfonate so that it exhibits liquid-like behavior and maintains its nanostructure in the liquid state, which can successfully overcome the problem of agglomeration of sodium lignin sulfonate particles in the prior art, and also avoid lignin dependence on special solvents when used, thereby avoiding harm to the environment.

[0007] Furthermore, the concept of the present invention is to provide a lignin soft solid, specifically, the obtained liquefied lignin is added to the powder raw materials of cellulose and sodium lignin sulfonate, and the mixture is fully stirred and mixed to obtain a lignin soft solid. The soft solid has good engineering mechanical properties and has broad industrial application prospects.

[0008] In view of the above concept, the present invention realizes the above concept through the following specific scheme. The present invention provides a method for preparing liquefied lignin, comprising the following steps:

[0009] 1) dissolving the sulfonated modified lignin and the quaternary ammonium salt in water respectively, and stirring for a certain period of time to obtain the sulfonated modified lignin solution and the quaternary ammonium salt solution;

[0010] 2) The sulfonated modified lignin solution obtained in step 1) is mixed with the quaternary ammonium salt solution, and after stirring for a certain period of time, the reactant is dried, and the viscous liquid on the upper layer of the reactant is taken, which is the quasi-liquefied lignin.

[0011] Wherein, the sulfonated modified lignin is sodium lignin sulfonate;

[0012] The quaternary ammonium salt is nonylphenol polyoxyethylene ether quaternary ammonium salt.

[0013] Furthermore, the number of ether bonds in the molecular chain of the nonylphenol polyoxyethylene ether quaternary ammonium salt is 15-70;

[0014] It should be noted that the number of ether bonds in the nonylphenol polyoxyethylene ether quaternary ammonium salt can reflect the molecular weight of the quaternary ammonium salt. In the present invention, the key to the reaction is to use the quaternary ammonium salt to modify the surface of the sodium lignin sulfonate. Therefore, different quaternary ammonium salt specifications will affect the performance of the final product, the liquefied lignin.

[0015] Furthermore, the weight ratio of the sulfonated modified lignin to the quaternary ammonium salt is 1:0.5-1.5, preferably 1:0.5-1; more preferably 1:1;

[0016] It should be noted that the weight ratio of the sulfonated modified lignin to the quaternary ammonium salt disclosed in the present invention refers to the mass ratio of the quaternary ammonium salt used in step 1 to the sulfonated modified lignin, and also reflects the raw material ratio in the reaction system in step 2).

[0017] In the step 2), the temperature of the heating reaction is 50-70°C; preferably 55-65°C;

[0018] Furthermore, the reaction medium in step 2) is water; the reaction system comprises sulfonated modified lignin, quaternary ammonium salt and water.

[0019] Furthermore, in the step 1), the weight percentage concentration of the sulfonated modified lignin in the sulfonated modified lignin solution is 3.5wt%-6wt%;

[0020] Furthermore, the weight percentage concentration of the quaternary ammonium salt in the quaternary ammonium salt solution in step 1) is 3.5wt%-6wt%;

[0021] It should be noted that in step 1), the proportion of the solute in the sulfonated modified lignin solution and the quaternary ammonium salt solution is mainly determined by mass. In this step, the solute sulfonated modified lignin and the quaternary ammonium salt are completely dissolved as much as possible, but the possibility that the solute is not completely dissolved is not excluded.

[0022] In another embodiment, the present invention further provides a lignin soft solid, wherein the preparation method of the lignin soft solid is to mix the liquefied lignin with sodium lignin sulfonate and cellulose to obtain the lignin soft solid;

[0023] Wherein, the mass ratio of the quasi-liquefaction lignin: sodium lignosulfonate: cellulose is 3-6:2-4:1-3: preferably 5:3:2;

[0024] Furthermore, the cellulose is microcrystalline cellulose;

[0025] Furthermore, the liquefied lignin is mixed with sodium lignin sulfonate and cellulose until there is no color difference, thus obtaining a lignin soft solid.

[0026] Compared with the prior art, the present invention first provides a quasi-liquefaction wood material, which uses sulfonated modified lignin and quaternary ammonium salt to react in a mixed manner to change the rheological properties of the lignin material, so that the lignin material has quasi-liquefaction properties, which is helpful for subsequent processing; in addition, the prepared quasi-liquefaction lignin is used as a raw material, which is mixed with sodium lignin sulfonate and cellulose to obtain a lignin soft solid, wherein the soft solid molecules are tightly bound by hydrogen bonds, and the quasi-liquefaction lignin promotes close contact between the components, so that the components are tightly adhered together. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The infrared spectra of liquefied sodium lignin sulfonate (LigFS), sodium lignin sulfonate (LS), quaternary ammonium salt (PEG-STA), and sodium lignin sulfonate / quaternary ammonium salt mixture;

[0028] Figure 2 This is the SEM image of lignin soft solid;

[0029] Figure 3 is the SEM image of the lignin composite material;

[0030] Figure 4 Mechanical properties diagram of lignin composites prepared from liquefied lignin of different chain lengths;

[0031] Figure 5 This is a mechanical property diagram of the lignin composite material prepared from liquefied lignin of nonylphenol polyoxyethylene ether quaternary ammonium salt 1820 with different contents in the present invention;

[0032] Figure 6 This is a test diagram of the recyclability of the cellulose composite material of the present invention. DETAILED DESCRIPTION

[0033] In order to enable those skilled in the art to better understand the technical solution of the present disclosure, the present disclosure is described in detail, clearly and completely in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present disclosure and are not used to limit the present disclosure.

[0034] This embodiment provides a method for preparing liquefiable lignin, comprising the following steps:

[0035] 1) dissolving the sulfonated modified lignin and the quaternary ammonium salt in water respectively, and stirring for a certain period of time to obtain the sulfonated modified lignin solution and the quaternary ammonium salt solution;

[0036] In the reaction system in step 1), the sulfonated lignin has a variety of functional groups, including hydroxyl, carboxyl, sulfonic acid, etc., which provide enough reaction sites for the reaction. At the same time, due to the introduction of a variety of hydrophilic groups, the water solubility of the material is greatly improved;

[0037] In addition, for quaternary ammonium salt solution, due to its positive charge property and the selection of functional groups on the quaternary ammonium salt, there is a reaction basis between sulfonated modified lignin and quaternary ammonium salt. At the same time, quaternary ammonium salt has greater solubility and provides a basis for preparing fluid-like materials. Based on this, it is expected to obtain liquefied lignin and improve the dispersion and interface properties of lignin.

[0038] 2) The sulfonated modified lignin solution obtained in step 1) is mixed with the quaternary ammonium salt solution, and after stirring for a certain period of time, the reactant is dried, and the viscous liquid on the upper layer of the reactant is taken, which is the quasi-liquefied lignin.

[0039] In step 2), since step 1) promotes the dissolution of the sulfonated modified lignin and the quaternary ammonium salt by heating, stirring and the like, support is provided for mixing the sulfonated modified lignin solution and the quaternary ammonium salt solution in step 2) and allowing them to react rapidly, and the sulfonated modified lignin and the quaternary ammonium salt have the same solvent, and the solution is not prone to interfacial reaction and deposition after mixing; in addition, the raw materials react at a high temperature so that the sulfonated modified lignin and the quaternary ammonium salt can be fully mixed and reacted fully;

[0040] Furthermore, the sulfonated modified lignin is sodium lignin sulfonate;

[0041] The quaternary ammonium salt is nonylphenol polyoxyethylene ether quaternary ammonium salt;

[0042] Among the reaction raw materials, the sulfonated modified lignin selected by the present invention is sodium lignin sulfonate, which has multiple hydroxyl groups, carboxyl groups and sulfonic acid groups. The selected nonylphenol polyoxyethylene ether quaternary ammonium salt is a surfactant, which can fully improve the surface properties of sodium lignin sulfonate. At the same time, the nonylphenol polyoxyethylene ether quaternary ammonium salt has a positive charge and can be fully and quickly combined with the sulfonated modified lignin. In addition, the polyether structure on the nonylphenol polyoxyethylene ether quaternary ammonium salt can be hydrogen-bonded with the corresponding groups on the sulfonated modified lignin.

[0043] Further, the number of ether bonds in the molecular chain of the nonylphenol polyoxyethylene ether quaternary ammonium salt is 15-70, preferably the number of ether bonds in the molecular chain of the nonylphenol polyoxyethylene ether quaternary ammonium salt is 20-70, and more preferably the number of ether bonds in the molecular chain of the nonylphenol polyoxyethylene ether quaternary ammonium salt is 20 or 70;

[0044] It should be noted that the nonylphenol polyoxyethylene ether quaternary ammonium salts selected in the embodiments of the present invention are nonylphenol polyoxyethylene ether quaternary ammonium salt 1815, nonylphenol polyoxyethylene ether quaternary ammonium salt 1820, nonylphenol polyoxyethylene ether quaternary ammonium salt 1830, nonylphenol polyoxyethylene ether quaternary ammonium salt 1860, and nonylphenol polyoxyethylene ether quaternary ammonium salt 1870; wherein the last two digits of different models represent the number of ether bonds, such as nonylphenol polyoxyethylene ether quaternary ammonium salt 1815 represents that there are 15 ether bonds in the quaternary ammonium salt, and nonylphenol polyoxyethylene ether quaternary ammonium salt 1820 represents that there are 20 ether bonds in the quaternary ammonium salt. In subsequent specific embodiments, those skilled in the art determine the number of ether bonds in the quaternary ammonium salt according to the specific model of the quaternary ammonium salt.

[0045] The number of ether bonds in the quaternary ammonium salt of polyoxyethylene phenol ether can reflect the molecular weight of the quaternary ammonium salt. In the present invention, different types of quaternary ammonium salts will affect the performance of the final product, the liquefied lignin. The quaternary ammonium salts with different molecular chain lengths have different coating and reaction degrees for the sulfonated modified lignin, which will eventually change the performance of the liquefied lignin prepared by the present invention.

[0046] Furthermore, the weight ratio of the sulfonated modified lignin to the quaternary ammonium salt is 1:0.5-1.5, preferably 1:0.5-1; more preferably 1:1;

[0047] In the step 2), the reaction temperature is 50-70°C; preferably 55-65°C;

[0048] In the reaction system of the present invention, although the raw material nonylphenol polyoxyethylene ether quaternary ammonium salt is a surfactant, in the system of the present invention, the nonylphenol polyoxyethylene ether quaternary ammonium salt is more of a reaction raw material. At the same time, the surface energy improvement performance and the reaction performance of the special structure of the nonylphenol polyoxyethylene ether quaternary ammonium salt are utilized, which is the basis for the reaction with lignin; therefore, the amount of the nonylphenol polyoxyethylene ether quaternary ammonium salt used in the present invention is much higher than the conventional amount used as a surfactant.

[0049] Furthermore, the reaction medium in step 1 (comprising sulfonated modified lignin, quaternary ammonium salt and water) is water; the reaction system comprises

[0050] Furthermore, the weight percentage concentration of the sulfonated modified lignin in the sulfonated modified lignin solution in step 1) is 3.5wt%-6wt%, preferably 4.5%;

[0051] Furthermore, the weight percentage concentration of the quaternary ammonium salt in the quaternary ammonium salt solution in step 1) is 3.5wt%-6wt%, preferably 4.5%.

[0052] In addition, this embodiment also provides a lignin soft solid, and the preparation method of the lignin soft solid is to mix the liquefied lignin with sodium lignin sulfonate and cellulose to obtain the lignin soft solid;

[0053] Specifically, the mass ratio of the liquefied lignin: sodium lignosulfonate: cellulose is 3-6:2-4:1-3: preferably 5:3:2;

[0054] In another embodiment, the lignin soft solid is shaped, cured, and subjected to high temperature treatment to obtain a lignin composite material;

[0055] Specifically, the present invention provides the following embodiments to fully illustrate the scheme of the present invention;

[0056] Example 1

[0057] Preparation of liquefiable lignin

[0058] Step 1: Sodium lignin sulfonate and nonylphenol polyoxyethylene ether quaternary ammonium salt 1820 are dissolved in the same amount of water, wherein the sodium lignin sulfonate accounts for 4.5% of the sodium sulfonate solution, and heated and stirred for 4 hours; wherein the weight ratio of sodium lignin sulfonate to nonylphenol polyoxyethylene ether quaternary ammonium salt is set to 1:0.1, 1:0.5, 1:1 and 1:1.5 respectively.

[0059] Step 2: After sufficient stirring, the two solutions were mixed and heated and stirred for 12 hours at a reaction temperature of 60° C. until the reaction was complete to obtain a mixed solution;

[0060] Step 3, drying the mixed solution in an oven for 12 hours to obtain a product;

[0061] Under the variable weight ratio of sodium lignin sulfonate and nonylphenol polyoxyethylene ether quaternary ammonium salt set in Example 1, when the weight ratio of sodium lignin sulfonate and nonylphenol polyoxyethylene ether quaternary ammonium salt is 1:0.1, the final product obtained is blocky, and it is difficult to see that a liquefied substance is obtained; when the weight ratio is 1:0.5-1.5, liquefied lignin can be obtained, but when the amount of quaternary ammonium salt continues to increase, the amount of fluid-like lignin is not significantly increased, but the cost is high due to the increased use of quaternary ammonium salt.

[0062] Example 2

[0063] Preparation of liquefiable lignin

[0064] Step 1, first dissolve sodium lignin sulfonate and nonylphenol polyoxyethylene ether quaternary ammonium salt 1820 in the same amount of water, wherein the gram weight ratio of sodium lignin sulfonate and nonylphenol polyoxyethylene ether quaternary ammonium salt is 1:1, and heat and stir for 4 hours; wherein the weight percentage concentration of sodium lignin sulfonate in the sodium sulfonate solution is 0.5%, 1%, 2%, 4%, 4.5%, 6%, and 7%.

[0065] Step 2: After sufficient stirring, the two solutions were mixed and heated and stirred for 12 hours at a reaction temperature of 60° C. until the reaction was complete to obtain a mixed solution;

[0066] Step 3, drying the mixed solution in an oven for 12 hours to obtain a product;

[0067] In Example 2, by controlling the concentration of the raw materials and observing the degree of reaction, from the concentration range of 0.5% to 2%, due to the low concentration of the raw materials, it is difficult to observe the acquisition of liquefied products in the final reaction product. This may be due to the fact that when the concentration is low, the reaction is not sufficient, so that the modification of lignin by quaternary ammonium salt requires more time, and since the reaction is generally balanced, it is not conducive to the modification of lignin at too low a concentration; in addition, we also found that when the concentration is further increased, the raw materials will be unevenly dispersed, which is also disadvantageous to the reaction.

[0068] In order to characterize the characteristics of liquefied sodium lignin sulfonate (LigFS) during the reaction process, the infrared spectra of liquefied sodium lignin sulfonate (LigFS), sodium lignin sulfonate (LS), quaternary ammonium salt (PEG-STA), and sodium lignin sulfonate / quaternary ammonium salt mixture were tested. Figure 1Among them, the sodium lignin sulfonate / quaternary ammonium salt mixture is a simple physical mixture and no reaction is carried out; it should also be noted that the nonylphenol polyoxyethylene ether quaternary ammonium salt 1820, which is labeled as PEG-STA-20, is used in this test;

[0069] Among them, Figure 1 , 3403cm -1 (OH stretching vibration), 1410cm -1 (-SO 3- stretching vibration), 1572cm -1 (aromatic ring C=C stretching vibration) is the characteristic peak of sodium lignin sulfonate. The quaternary ammonium salt of nonylphenol polyoxyethylene ether (PEG-STA) is at 2923cm -1 (-CH 3 CH symmetric stretching vibration), 2853cm -1 (-CH 2 A series of characteristic peaks appeared at the CH symmetric stretching vibration, in addition to the peaks at 1097 cm -1 (COC asymmetric stretching vibration) and 1453cm -1 (NH + Two strong vibration peaks appeared at the in-plane deformation vibration of the liquefied lignin. In the infrared curve of the liquefied lignin, the sulfonate group (-SO 3 - stretching vibration) disappears, and the aromatic ring C=C stretching vibration decreases from 1572cm -1 The absorption band of OH becomes stronger when it moves to 1642 cm-1, and the absorption band of COC increases from 1097 cm-1 to 1642 cm-1. -1 Moved to 1086cm -1 , indicating that ionic reaction and hydrogen bonding occurred between sodium lignin sulfonate and quaternary ammonium salt, proving the successful synthesis of liquefied lignin.

[0070] Example 3

[0071] Effects of different quaternary ammonium salt specifications on liquefiable lignin.

[0072] Based on the parameters of the raw materials determined in Examples 1-2, the invention also provides a liquefied lignin-based soft solid and a composite material prepared from the soft solid. The specific operation is as follows:

[0073] Step 1: Prepare the raw material solution

[0074] First, sodium lignin sulfonate and nonylphenol polyoxyethylene ether quaternary ammonium salt are dissolved in the same amount of water, wherein the weight ratio of sodium lignin sulfonate and nonylphenol polyoxyethylene ether quaternary ammonium salt is 1:1, sodium lignin sulfonate accounts for 4.5% in the sodium lignin sulfonate solution, and quaternary ammonium salt accounts for 4.5% in the quaternary ammonium salt solution; adjust the quaternary ammonium salt with different polyether contents, and the specific adjustment is shown in Table 1;

[0075] Table 1 Proportion of each component of liquefied lignin prepared by quaternary ammonium salts with different chain lengths

[0076] Quaternary ammonium salt types Sodium lignin sulfonate(g) Quaternary ammonium salt mass (g) 1815 5 5 1820 5 5 1830 5 5 1860 5 5 1870 5 5

[0077] Step 2: Preparation of liquefied lignin

[0078] After sufficient stirring, the two solutions were mixed and heated and stirred for 12 hours at a reaction temperature of 85°C until the reaction was complete to obtain a mixed solution; the mixed solution was dried in an oven for 12 hours to obtain liquefied lignin;

[0079] Step 3, a lignin soft solid, wherein the preparation method of the lignin soft solid is to mix the liquefied lignin with sodium lignin sulfonate and cellulose to obtain the lignin soft solid;

[0080] The cellulose is microcrystalline cellulose; the mass ratio of quasi-liquefaction lignin: sodium lignin sulfonate: cellulose is 3-6:2-4:1-3: specifically, the mass ratio in this embodiment is 5:3:2; the quasi-liquefaction lignin, sodium lignin sulfonate and cellulose are mixed until there is no color difference, that is, a lignin soft solid is obtained. The specific parameters are shown in Table 2;

[0081] Table 2 Proportion of each component in composite materials prepared from liquefied lignin of different chain lengths

[0082]

[0083] Note: The data in brackets are the percentage of raw materials.

[0084] Step 4 Preparation of lignin composite material

[0085] The lignin soft solid obtained in step 3 is dried and solidified to obtain a composite material.

[0086] Among them, the quaternary ammonium salt in step 3 and the scheme in which the quaternary ammonium salt is nonylphenol polyoxyethylene ether quaternary ammonium salt 1820 are selected for scanning electron microscopy test to observe the apparent properties of the soft solid and lignin composite materials. Figure 2 This is the SEM image of lignin soft solid. Figure 3 is the SEM image of the lignin composite material;

[0087] Specifically, in order to observe the surface morphology of the composite material, Figure 2 The microstructure of the lignin soft solid was obtained by scanning electron microscopy (SEM). It can be observed that the quasi-liquefied lignin is evenly dispersed in the system. Due to the effect of hydrogen bonding, the quasi-liquefied lignin firmly binds the components together. At the same time, the presence of quaternary ammonium salt on the quasi-liquefied lignin gives the composite material good flexibility, and the composite material has excellent plasticity.

[0088] Figure 3 This is the SEM image of the lignin composite material. It can be observed that due to the dispersion and adhesion of the quasi-liquefied lignin, when the quasi-liquefied lignin is completely dried, the quasi-liquefied lignin is fixed, and along with the evaporation of water, the composite material is densified to form fine wrinkles, which makes the morphology of the composite material fixed. Through the synergistic effect of adhesion, intermolecular force and densification, the composite material exhibits high strength.

[0089] In addition, this embodiment tests the mechanical properties of the lignin composite material obtained in step 4. Figure 4 , which is a mechanical property diagram of lignin composites prepared from liquefied lignin of different chain lengths. By changing the length of the organic chain of the liquefied lignin, the liquefied lignin of different chain lengths is used to prepare lignin composites, and then a tensile test is performed. It can be seen from the figure that the lignin composite prepared from nonylphenol polyoxyethylene ether quaternary ammonium salt 1820 has the strongest mechanical properties. This is because with the increase of chain length, the liquefied lignin has better fluidity, more uniform contact with sodium lignin sulfonate and cellulose, and increases the bonding area and interface compatibility. The significant decrease in the mechanical properties of the liquefied lignin 1860 is due to the substantial increase in organic chains, which leads to self-entanglement between chains and reduces fluidity. Thereby reducing the interface compatibility between lignin and cellulose. The mechanical properties of the liquefied lignin 1870 have been slightly improved because the content of organic chain 1870 in the liquefied lignin 1870 is high, which increases the adhesion between lignin and cellulose, thereby improving the mechanical properties.

[0090] Example 4

[0091] Based on Example 3, in order to further verify the performance of the lignin composite material, the mass ratio of quasi-liquefied lignin: sodium lignosulfonate: cellulose in step 3 of Example 3 was adjusted, and a lignin composite material was obtained based on this. The specific adjustment design is shown in Table 3;

[0092] Table 3 Proportion of each component in composite materials prepared with different contents of 1820 liquefied lignin

[0093]

[0094] In the embodiments, when the content of quasi-liquefaction lignin is too low, the formed lignin composite material has a loose structure and cannot be formed, and when the content is too high, the lignin composite material is too viscous and cannot be formed.

[0095] This example tests the mechanical properties of the obtained lignin composite material. The specific results are shown in Figure 5

[0096] Figure 5 The figure is a mechanical property diagram of the lignin composite material prepared from the liquefied lignin of nonylphenol polyoxyethylene ether quaternary ammonium salt 1820 with different contents of the present invention. The tensile test is performed on the liquefied lignin 1820 with different contents. It can be seen from the figure that when the content of the liquefied lignin 1820 increases, the mechanical properties gradually increase. It means that with the increase of the liquefied lignin, the adhesion between sodium lignin sulfonate, cellulose and the liquefied lignin is stronger, the intermolecular force is more, and the degree of densification is stronger, so that the mechanical properties of the lignin composite material are gradually enhanced. The difference in mechanical properties is due to the deviation caused by manual shaping, but it does not affect the comparative experiment of samples from the same batch.

[0097] Example 5

[0098] Recycling performance of lignin composites,

[0099] The dried lignin composite material is ground to obtain a powdered composite material, the powdered composite material is recovered, a certain amount of water is added, and the mixture is stirred again to obtain a soft solid, and the soft solid is dried and solidified to obtain a formed composite material.

[0100] For detailed process, see Figure 6 , Figure 6 This is a test diagram of the recyclability of the cellulose composite material of the present invention. The dried lignin composite material is ground and the powdered composite material is easy to recycle and reuse. At the same time, it can be observed that the powder can be added with water for secondary processing, and a strip composite material can be obtained by drying.

[0101] It should be noted that the various embodiments of the present application can be arbitrarily combined into a new embodiment if the solutions do not conflict and the technical solutions can coexist.

[0102] The present application is described in detail above. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the present application and its core ideas. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present application, several improvements and modifications can be made to the present application, and these improvements and modifications also fall within the scope of protection of the claims of the present application.

Claims

1. A method for preparing liquefiable lignin, comprising the following steps: 1) dissolving the sulfonated modified lignin and the quaternary ammonium salt in water respectively, and stirring for a certain period of time to obtain the sulfonated modified lignin solution and the quaternary ammonium salt solution; 2) The sulfonated modified lignin solution obtained in step 1) is mixed with the quaternary ammonium salt solution, and after stirring for a certain period of time, the reactant is dried, and the viscous liquid on the upper layer of the reactant is taken, which is the quasi-liquefied lignin.

2. The method for preparing liquefiable lignin according to claim 1, characterized in that: The sulfonated modified lignin is sodium lignin sulfonate; The quaternary ammonium salt is nonylphenol polyoxyethylene ether quaternary ammonium salt.

3. The method for preparing liquefiable lignin according to claim 2, characterized in that: The number of ether bonds in the molecular chain of the nonylphenol polyoxyethylene ether quaternary ammonium salt is 15-70.

4. The method for preparing liquefiable lignin according to claim 3, characterized in that: The weight ratio of the sulfonated modified lignin to the quaternary ammonium salt is 1:0.5-1.5, preferably 1:0.5-1; more preferably 1:

1.

5. The method for preparing liquefiable lignin according to claim 4, characterized in that: In the step 2), the temperature of the heating reaction is 50-70°C.

6. The method for preparing liquefiable lignin according to claim 5, characterized in that: The weight percentage concentration of the sulfonated modified lignin solution in step 1) is 3.5wt%-6wt%; The weight percentage concentration of the quaternary ammonium salt solution in step 1) is 3.5wt%-6wt%.

7. The method for preparing liquefiable lignin according to any one of claims 1 or 5, characterized in that: The weight percentage concentration of the sulfonated modified lignin solution in step 1) is 4.5%; The weight percentage concentration of the quaternary ammonium salt solution in step 1) is 4.5%.

8. A liquefied lignin, characterized in that: It is prepared by the method according to any one of claims 1 to 7.

9. A method for preparing a lignin composite material, characterized in that Using the quasi-liquefaction lignin as claimed in claim 8, the preparation method comprises: mixing the quasi-liquefaction lignin with sodium lignin sulfonate and cellulose to obtain a lignin soft solid; shaping and curing the lignin soft solid to obtain a lignin composite material.

10. The method for preparing the lignin composite material according to claim 9, characterized in that: The mass ratio of the quasi-liquefied lignin: sodium lignosulfonate: cellulose is 5:2:3; The cellulose is microcrystalline cellulose.

Citation Information

Cited By

  • A high-performance fluid-based fiber aerogel, its preparation method and application

    CN122665588A