Structural color visualization and electric signal digitization coupled strain sensing material and preparation method and application thereof

Through the co-assembly technology of cellulose nanocrystals and MXene, the problem of difficult balance between mechanical properties and tensile properties of polysaccharide hydrogel films is solved, the structural color contrast is improved, and the strain transmission of structural color visualization and digital coupling of electrical signals is realized. Sensory materials, suitable for intelligent motion monitoring and human-computer interaction fields.

CN119081150APending Publication Date: 2024-12-06CARBON HENG (CHONGQING) BIOMASS NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410907482.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The mechanical properties and tensile properties of traditional polysaccharide hydrogel films are difficult to balance. The structural color contrast of cellulose nanocrystalline chiral array hydrogel films is insufficient, which limits its application potential in mechanical stimulation response sensors.

Method used

By preparing the co-assembly of cellulose nanocrystalline suspension and MXene suspension, using polyvinyl alcohol as a regulator, a cellulose nanocrystalline chiral array structure and MXene conductive pathway are formed, and the structure color visualization and digital coupling of electrical signals are achieved by combining alkali treatment. strain sensing material.

Benefits of technology

It has achieved improvements in the mechanical and conductive properties of the material, significantly improved the structural color contrast, given it application potential in the fields of intelligent motion monitoring and human-machine interaction, and provided a new direction for wearable devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081150A_ABST
    Figure CN119081150A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a structural color visualization and electric signal digitization coupled strain sensing material. The preparation method comprises the following steps: S1, preparing a cellulose nanocrystal (CNC) suspension; s2, a CNC chiral array and MXene co-assembly material is prepared; s3, preparing a structural color visualization and electric digitization strain sensor material; through a co-assembly strategy of a flexible polymer chain, functional nanoparticles and CNC particles forming a structural color array, flexible polymer co-assembly is introduced to lay a mechanical foundation of strain sensing, and one-dimensional rod-shaped CNC and two-dimensional MXene are regulated and controlled to be mutually coordinated and compatible to synchronously construct the structural color array and a conductive path. Therefore, correlation between structural color and resistivity change and the tensile strain process is established, coupling of strain sensing visualization and electric signal quantification correlation is realized, and technical methods and material types of human motion monitoring and the like in the field of intelligent sensing equipment are expected to be enriched.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of biomass polymer nanocomposite materials, and relates to a strain sensing material coupled with structural color visualization and electric signal digitization, and a preparation method and application thereof. Background Art

[0002] Polysaccharides are a class of natural polymers with advantages such as wide sources, good biocompatibility and environmental friendliness. They have great application potential in the fields of sensors, ion conductors and biomedicine. However, polysaccharides such as cellulose, chitin and similar chitosan are difficult to dissolve in common organic solvents and water, which limits their practical applications. As an important application form, polysaccharide-based hydrogels usually need to find a balance between hardness and stretchability. When flexible polymers are used as the matrix, although hydrogels with good stretchability can be obtained, this is mainly due to the matrix polymer itself, and polysaccharides mainly play a reinforcing or toughening role. On the contrary, when polysaccharides are used as the main matrix of hydrogels (the content exceeds 50%), the resulting hydrogels have good mechanical strength, but their tensile properties are often poor, which limits their use in real life.

[0003] The structural color changes of cellulose nanocrystal-based chiral array hydrogel films during stretching provide new possibilities for their application in the field of sensors. This structural color change not only provides an intuitive way to perceive and respond to external mechanical stimuli, but also enables the hydrogel film to be used as a visual sensor in a variety of application scenarios. However, the lack of structural color contrast makes it difficult to clearly distinguish the structural color changes caused by strain. This limitation is not conducive to its potential application in mechanical stimulus response sensors.

[0004] As a new type of two-dimensional transition metal carbide and nitride, MXene has attracted much attention due to its excellent physical and chemical properties. Due to its rich oxygen or hydroxyl terminal surface and complete metal atomic layer, MXene can interact with most biomolecules through hydrogen bonds, van der Waals forces, electrostatic interactions, coordination bonds, etc., which makes it a unique nanobiological unit in the biosensor structure. Compared with graphene oxide, MXene has obvious advantages in light absorption from visible light to near-infrared region. Therefore, a visual and digital strain sensing material composited with MXene and cellulose nanocrystals is needed. Summary of the invention

[0005] In view of this, one of the objects of the present invention is to provide a method for preparing a strain sensing material with structural color visualization coupled with digitalization of electrical signals, so as to solve the problem that it is difficult to balance the mechanical properties and tensile properties of traditional polysaccharide-based hydrogel membranes, and the problem that the structural color contrast presented by the mechanical stimulation response of cellulose nanocrystal-based chiral array hydrogel membranes is insufficient; a second object of the present invention is to provide a strain sensing material product prepared by a method for preparing a strain sensing material with structural color visualization coupled with digitalization of electrical signals; a third object of the present invention is to provide the application of the strain sensing material product with structural color visualization coupled with digitalization of electrical signals in the field of visualization and digital sensing.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] A method for preparing a strain sensing material with structural color visualization and electrical signal digital coupling comprises the following steps:

[0008] S1. Preparation of cellulose nanocrystal suspension: treating biomass from different cellulose sources with sulfuric acid to obtain a one-dimensional rod-shaped cellulose nanocrystal (CNC) suspension with high aspect ratio, high specific surface area and excellent photoluminescence performance, and concentrating it to 2-8 wt% by rotary evaporation;

[0009] S2. Preparation of CNC chiral array and MXene co-assembled material: In order to adjust the proportion of each component in the co-assembled material to adjust the mechanical properties of the material, 10-20% polyvinyl alcohol (PVA) solution, cellulose nanocrystal suspension prepared in step S1 and MXene suspension are mixed in a mass ratio of (10-50):80:(10-15), and magnetically stirred at room temperature for 5 hours to obtain a uniform dispersion; the above dispersion is then placed in an ice water bath and ultrasonically treated with an ultrasonic cleaner for 5-10 minutes to induce the one-dimensional rod-shaped end of the CNC to enter the MXene layer, forming a "needle tip prying" effect, and cellulose nanocrystal chiral array co-assembled material is obtained by evaporation-induced self-assembly at room temperature. Evaporation-induced self-assembly at room temperature helps to obtain the cellulose nanocrystal chiral array structure of the co-assembled material and take into account the formation of MXene conductive paths;

[0010] S3. Preparation of structural color visualization and electrical digital strain sensor material: The cellulose nanocrystal chiral array co-assembled material prepared in step S2 is subjected to alkali treatment at room temperature for 1 hour, and then washed with deionized water until neutral to obtain a structural color visualization and electrical digital strain sensor material.

[0011] Furthermore, in step S1, the cellulose nanocrystals are derived from one or more mixtures of cotton, coniferous wood, flax, ascidian, cotton stalks or bagasse.

[0012] Furthermore, in step S1, the length of the cellulose nanofibers ranges from 100 to 700 nm, and the width ranges from 2 to 12 nm; the concentration of the cellulose nanofiber dispersion is 0.1 to 1 wt %.

[0013] Furthermore, the specification of the polyvinyl alcohol in step S2 is PVA-1788, and the alcoholysis degree is 87-89.

[0014] Furthermore, in step S2, the ultrasonic power in the ice bath environment is 50-400 W, which is conducive to forming a "needle tip prying" effect that induces the one-dimensional rod-shaped end of the CNC to enter the MXene layer, thereby improving the dispersion stability in the MXene suspension, the uniformity of distribution within the material, and the reliability of forming a conductive path.

[0015] Further, the preparation method of the MXene suspension in step S2 is: after 1.0-4.0g of MXene powder is slowly added to a mixed solution containing 20-60mL 7-9mol / L HCl and 3.0-5.0g LiF, the layered MXene is prepared by continuous stirring at 40°C for 48h; the resulting solution is then centrifuged and washed 3 times with 4mol / L HCl; and then washed several times with deionized water until the pH of the supernatant is close to neutral. The precipitate obtained by centrifugation is dispersed in a silk-mouth bottle filled with deionized water, and then ultrasonically treated in an ice bath for 1h; finally, the solution is centrifuged at 5000rpm for 0.5h, and the upper layer of liquid is collected to obtain a MXene suspension containing a few-layer MXene nanosheets.

[0016] Furthermore, the solid content of the MXene suspension in step S2 is 0.02-0.1 wt %, which ensures that the MXene forms a conductive pathway and its sensing response is linearly related to the sensitivity and slows down the agglomeration in the CNC / PVA assembly suspension.

[0017] Furthermore, the dispersion in step S2 is heated to 0.05-1.0 mL / (cm 2 ·day) evaporation-induced rate to self-assemble to ensure that the chiral array structure of cellulose nanocrystals and the MXene conductive pathway of the co-assembled material are obtained.

[0018] Furthermore, the concentration of the sodium hydroxide solution in step S3 is 1 to 3 mol / L.

[0019] The strain sensing material product is prepared according to the strain sensing material preparation method of coupling structural color visualization with electrical signal digitization.

[0020] The strain sensing material products that couple the above-mentioned structural color visualization with the digitalization of electrical signals are used in the fields of visualization and digital intelligent sensing, motion monitoring, and sensing equipment.

[0021] The beneficial effects of the present invention are:

[0022] 1. The strain sensing material coupled with structural color visualization and electrical signal digitization disclosed in the present invention is formed by adding 10% polyvinyl alcohol solution and MXene suspension to cellulose nanocrystal suspension to form an assembly precursor, using the self-assembly behavior of cellulose nanocrystals to prepare a membrane material with a chiral array structure, and then cross-linking the assembled membrane through alkali treatment to obtain a structural color visualization and electrical digitization strain sensor material. The structural color visualization and electrical digitization strain sensor material can meet both the mechanical performance requirements of daily sensing applications and the requirements of visualization and digital sensing functions.

[0023] 2. The strain sensing material with structural color visualization and digital coupling of electrical signals disclosed in the present invention can precisely control the structural color by adjusting the ratio of PVA to CNC. The introduction of an appropriate amount of MXene will not only not affect the chiral assembly, but also improve the structural color contrast. In addition, due to the hydrophilicity of CNC / PVA / MXene, the three can be evenly dispersed, which makes MXene evenly dispersed in the chiral array structure formed by CNC / PVA, prompting it to form a good conductive path, further enhancing the conductive properties of the material; at the same time, the cross-linking of the flexible polymer is achieved through alkali treatment, which significantly improves the tensile properties of the polysaccharide-based hydrogel and gives it the ability to respond to mechanical stimulation structural colors. The material prepared by this method has excellent conductive and mechanical properties while maintaining the structural color visualization characteristics, and is expected to be used in the field of intelligent sports equipment and for human training monitoring.

[0024] 3. The method for preparing the strain sensing material with structural color visualization and digital coupling of electrical signals disclosed in the present invention is to induce self-assembly of black conductive material MXene and biomass-derived nanoparticle cellulose nanocrystals through evaporation to prepare a membrane material containing a chiral array structure of cellulose nanocrystals, and then form a hydrogel membrane material through alkali treatment. The black conductive MXene not only gives the hydrogel film conductive properties, but also improves the color contrast, further enriching the structural color change effect of the hydrogel when stretched. The hydrogel can monitor the tiny movements of the human body and a wide range of daily activities in real time. In addition, the hydrogel film can be made into a capacitive pen that can write smoothly on the screen. It not only opens up new application possibilities for fields such as human-computer interaction and soft electronic skin, but also provides a new direction for the development of wearable devices.

[0025] Other advantages, objectives and features of the present invention will be described in the following description to some extent, and to some extent, will be obvious to those skilled in the art based on the following examination and study, or can be taught from the practice of the present invention. The objectives and other advantages of the present invention can be realized and obtained through the following description. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be described in detail below in conjunction with the accompanying drawings, wherein:

[0027] Figure 1 This is a scanning electron microscope image of a cross-section of a bio-based nanoparticle conductive chiral array hydrogel membrane material prepared in step S4 of Example 4 of the present invention;

[0028] Figure 2 This is an EDX spectrum diagram of the cross section of the bio-based nanoparticle conductive chiral array hydrogel film material prepared in step S4 of the fourth embodiment of the present invention, Figure 2 The upper left is a scanning electron microscope image of a cross-section of a bio-based nanoparticle conductive chiral array hydrogel film; Figure 2 The upper right shows the distribution of carbon; Figure 2 The lower left is the oxygen element distribution map; Figure 2 The lower right is the distribution diagram of titanium element; it shows that all components are evenly distributed in the material;

[0029] Figure 3 These are optical photographs of the bio-based nanoparticle conductive chiral array hydrogel film material prepared in step S3 of Example 4 of the present invention when the tensile strain is 40%, 80%, and 120% respectively;

[0030] Figure 4 Comparison diagram of stress-strain curves of bio-based nanoparticle conductive chiral array hydrogel film materials prepared in Examples 1 to 4 of the present invention with different amounts of polyvinyl alcohol (PVA) added;

[0031] Figure 5 (a) is the correlation between the relative resistance change and tensile strain of the flexible sensor based on the bio-based nanoparticle conductive chiral array hydrogel film material prepared in step S5 of Example 4 of the present invention;

[0032] Figure 5 (b) is a graph showing the relative resistance change of the flexible sensor based on the bio-based nanoparticle conductive chiral array hydrogel film material prepared in step S5 of Example 4 of the present invention after repeated loading and unloading for 200 times under 20% tensile strain;

[0033] Figure 6 (a) is a graph showing the relative resistance change of the flexible sensor based on the bio-based nanoparticle conductive chiral array hydrogel film material prepared in step S5 of Example 4 of the present invention when pressed by a finger;

[0034] Figure 6 (b) is a graph showing the relative resistance change of the flexible sensor based on the bio-based nanoparticle conductive chiral array hydrogel film material prepared in step S5 of Example 4 of the present invention when smiling;

[0035] Figure 6 (c) is a graph showing the relative resistance change of the flexible sensor based on the bio-based nanoparticle conductive chiral array hydrogel film material prepared in step S5 of Example 4 of the present invention when making a fist;

[0036] Figure 7 "Hello!" (left) and "Smile" (right) written on a tablet by a simple capacitive pen made of bio-based nanoparticle conductive chiral array hydrogel film material prepared in step S3 of comparative example 4 of the present invention;

[0037] Figure 8 This is a photograph of the bio-based nanoparticle chiral array hydrogel film material prepared in step S4 of comparative example 4 of the present invention after stretching, proving that the addition of black MXene can enhance the color contrast;

[0038] Fig. 9 These are photos of the cellulose nanocrystal chiral array co-assembly materials prepared in step S3 of Examples 1 to 4 of the present invention. From left to right, the amounts of PVA added are 1.0 g, 1.5 g, 2.0 g, and 2.5 g, respectively. DETAILED DESCRIPTION

[0039] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0040] Embodiment 1

[0041] The amount of PVA added was 1 g, and the mass ratios of PVA to CNC and MXene suspension were 20:80:13, respectively, denoted as CP 1.0 M.

[0042] A method for preparing a strain sensor for coupling structural color visualization with electrical signal digitization comprises the following steps:

[0043] S1. preparing a cellulose nanocrystal suspension hydrolyzed with sulfuric acid: extracting cellulose nanocrystals with a length of about 116 nm from cotton linters, uniformly dispersing the extracted cellulose nanocrystals, concentrating them into a 2 wt % cellulose nanocrystal suspension, and ultrasonically treating them for 5 min to obtain a uniformly dispersed cellulose nanocrystal suspension;

[0044] S2. Preparation of MXene suspension: First, 2.0 g of Ti3AlC2 powder was slowly added to a mixed solution containing 40.0 mL of 9 M HCl and 3.2 g of LiF to ensure adequate mixing. Next, the mixture was stirred at 40 ° C for 48 h to prepare layered MXene. After completion, the solid and liquid were separated by centrifugation, and then washed three times with 4 mol / L HCl solution to remove residual impurities. Continue to wash with deionized water multiple times until the pH value of the supernatant is close to neutral. Next, the centrifuged precipitate was redispersed in a silk-mouth bottle filled with deionized water and ultrasonically treated for 1 h under ice bath conditions to further disperse the MXene nanosheets. Finally, the upper layer of liquid was collected by centrifugation at a speed of 5000 rpm for 0.5 h to obtain a dispersion of monolayer MXene nanosheets. The solid content was measured to be 0.83 wt%.

[0045] S3, preparing cellulose nanocrystal chiral array co-assembly material: taking 20 mL of the aqueous suspension of cellulose nanocrystals after sulfuric acid-catalyzed hydrolysis in step S1, taking 1.0-2.5 g of 10% polyvinyl alcohol solution and 0.8 g of MXene suspension and adding them to the aqueous suspension of cellulose nanocrystals, stirring at room temperature for 4 h at 800 rpm in a stirrer to obtain an assembly precursor, and then placing it in a polystyrene culture dish with a diameter of 6 cm, and obtaining a cellulose nanocrystal chiral array co-assembly material by evaporation-induced self-assembly under ambient conditions;

[0046] S4. Preparation of structural color visualization and electrical digital strain sensor materials: The cellulose nanocrystal chiral array co-assembly material prepared in step S3 is soaked in a 3 mol / L NaOH solution at room temperature for 1 hour, and then washed with deionized water until neutral, and finally a bio-based nanoparticle conductive chiral array hydrogel membrane material is obtained;

[0047] S5. Preparation of flexible sensors with structural color visualization and electrical digital strain sensor materials: Cut the bio-based nanoparticle conductive chiral array hydrogel film material prepared in step S4 into strips with a length of 50.0 mm, a width of 10.0 mm, and a thickness of 0.02 mm, and wrap both ends of the strips with copper foil to ensure a close fit with the hydrogel film, then connect the copper foil to a wire and connect it to a multimeter to form a loop to form a flexible sensor.

[0048] Embodiment 2

[0049] The amount of PVA added was 1.5 g, and the mass ratios of PVA to CNC and MXene suspension were 30:80:13, respectively, denoted as CP 1.5 M.

[0050] A method for preparing a strain sensor for coupling structural color visualization with electrical signal digitization comprises the following steps:

[0051] S1. preparing a cellulose nanocrystal suspension hydrolyzed with sulfuric acid: extracting cellulose nanocrystals with a length of about 116 nm from cotton linters, uniformly dispersing the extracted cellulose nanocrystals, concentrating them into a 2 wt % cellulose nanocrystal suspension, and ultrasonically treating them for 5 min to obtain a uniformly dispersed cellulose nanocrystal suspension;

[0052] S2. Preparation of MXene suspension: First, 2.0 g of Ti3AlC2 powder was slowly added to a mixed solution containing 40.0 mL of 9 M HCl and 3.2 g of LiF to ensure adequate mixing. Next, the mixture was stirred at 40 ° C for 48 h to prepare layered MXene. After completion, the solid and liquid were separated by centrifugation, and then washed three times with 4 mol / L HCl solution to remove residual impurities. Continue to wash with deionized water multiple times until the pH value of the supernatant is close to neutral. Next, the centrifuged precipitate was redispersed in a silk-mouth bottle filled with deionized water and ultrasonically treated for 1 h under ice bath conditions to further disperse the MXene nanosheets. Finally, the upper layer of liquid was collected by centrifugation at a speed of 5000 rpm for 0.5 h to obtain a dispersion of monolayer MXene nanosheets. The solid content was measured to be 0.83 wt%.

[0053] S3, preparing cellulose nanocrystal chiral array co-assembly material: taking 20 mL of the aqueous suspension of cellulose nanocrystals after sulfuric acid-catalyzed hydrolysis in step S1, taking 1.0-2.5 g of 10% polyvinyl alcohol solution and 0.8 g of MXene suspension and adding them to the aqueous suspension of cellulose nanocrystals, stirring at room temperature for 4 h at 800 rpm in a stirrer to obtain an assembly precursor, and then placing it in a polystyrene culture dish with a diameter of 6 cm, and obtaining a cellulose nanocrystal chiral array co-assembly material by evaporation-induced self-assembly under ambient conditions;

[0054] S4. Preparation of structural color visualization and electrical digital strain sensor materials: The cellulose nanocrystal chiral array co-assembly material prepared in step S3 is soaked in a 3 mol / L NaOH solution at room temperature for 1 hour, and then washed with deionized water until neutral, and finally a bio-based nanoparticle conductive chiral array hydrogel membrane material is obtained;

[0055] S5. Preparation of flexible sensors with structural color visualization and electrical digital strain sensor materials: Cut the bio-based nanoparticle conductive chiral array hydrogel film material prepared in step S4 into strips with a length of 50.0 mm, a width of 10.0 mm, and a thickness of 0.02 mm, and wrap both ends of the strips with copper foil to ensure a close fit with the hydrogel film, then connect the copper foil to a wire and connect it to a multimeter to form a loop to form a flexible sensor.

[0056] Embodiment 3

[0057] The amount of PVA added was 2 g, and the mass ratios of PVA to CNC and MXene suspension were 40:80:13, respectively, denoted as CP 2.0 M.

[0058] A method for preparing a strain sensor for coupling structural color visualization with electrical signal digitization comprises the following steps:

[0059] S1. preparing a cellulose nanocrystal suspension hydrolyzed with sulfuric acid: extracting cellulose nanocrystals with a length of about 116 nm from cotton linters, uniformly dispersing the extracted cellulose nanocrystals, concentrating them into a 2 wt % cellulose nanocrystal suspension, and ultrasonically treating them for 5 min to obtain a uniformly dispersed cellulose nanocrystal suspension;

[0060] S2. Preparation of MXene suspension: First, 2.0 g of Ti3AlC2 powder was slowly added to a mixed solution containing 40.0 mL of 9 M HCl and 3.2 g of LiF to ensure adequate mixing. Next, the mixture was stirred at 40 ° C for 48 h to prepare layered MXene. After completion, the solid and liquid were separated by centrifugation, and then washed three times with 4 mol / L HCl solution to remove residual impurities. Continue to wash with deionized water multiple times until the pH value of the supernatant is close to neutral. Next, the centrifuged precipitate was redispersed in a silk-mouth bottle filled with deionized water and ultrasonically treated for 1 h under ice bath conditions to further disperse the MXene nanosheets. Finally, the upper layer of liquid was collected by centrifugation at a speed of 5000 rpm for 0.5 h to obtain a dispersion of monolayer MXene nanosheets. The solid content was measured to be 0.83 wt%.

[0061] S3, preparing cellulose nanocrystal chiral array co-assembly material: taking 20 mL of the aqueous suspension of cellulose nanocrystals after sulfuric acid-catalyzed hydrolysis in step S1, taking 1.0-2.5 g of 10% polyvinyl alcohol solution and 0.8 g of MXene suspension and adding them to the aqueous suspension of cellulose nanocrystals, stirring at room temperature for 4 h at 800 rpm in a stirrer to obtain an assembly precursor, and then placing it in a polystyrene culture dish with a diameter of 6 cm, and obtaining a cellulose nanocrystal chiral array co-assembly material by evaporation-induced self-assembly under ambient conditions;

[0062] S4. Preparation of structural color visualization and electrical digital strain sensor materials: The cellulose nanocrystal chiral array co-assembly material prepared in step S3 is soaked in a 3 mol / L NaOH solution at room temperature for 1 hour, and then washed with deionized water until neutral, and finally a bio-based nanoparticle conductive chiral array hydrogel membrane material is obtained;

[0063] S5. Preparation of flexible sensors with structural color visualization and electrical digital strain sensor materials: Cut the bio-based nanoparticle conductive chiral array hydrogel film material prepared in step S4 into strips with a length of 50.0 mm, a width of 10.0 mm, and a thickness of 0.02 mm, and wrap both ends of the strips with copper foil to ensure a close fit with the hydrogel film, then connect the copper foil to a wire and connect it to a multimeter to form a loop to form a flexible sensor.

[0064] Embodiment 4

[0065] The amount of PVA added was 2.5 g, and the mass ratios of PVA to CNC and MXene suspension were 50:80:13, respectively, denoted as CP 2.5 M.

[0066] A method for preparing a strain sensor for coupling structural color visualization with electrical signal digitization comprises the following steps:

[0067] S1. preparing a cellulose nanocrystal suspension hydrolyzed with sulfuric acid: extracting cellulose nanocrystals with a length of about 116 nm from cotton linters, uniformly dispersing the extracted cellulose nanocrystals, concentrating them into a 2 wt % cellulose nanocrystal suspension, and ultrasonically treating them for 5 min to obtain a uniformly dispersed cellulose nanocrystal suspension;

[0068] S2. Preparation of MXene suspension: First, 2.0 g of Ti3AlC2 powder was slowly added to a mixed solution containing 40.0 mL of 9 M HCl and 3.2 g of LiF to ensure adequate mixing. Next, the mixture was stirred at 40 ° C for 48 h to prepare layered MXene. After completion, the solid and liquid were separated by centrifugation, and then washed three times with 4 mol / L HCl solution to remove residual impurities. Continue to wash with deionized water multiple times until the pH value of the supernatant is close to neutral. Next, the centrifuged precipitate was redispersed in a silk-mouth bottle filled with deionized water and ultrasonically treated for 1 h under ice bath conditions to further disperse the MXene nanosheets. Finally, the upper layer of liquid was collected by centrifugation at a speed of 5000 rpm for 0.5 h to obtain a dispersion of monolayer MXene nanosheets. The solid content was measured to be 0.83 wt%.

[0069] S3, preparing cellulose nanocrystal chiral array co-assembly material: taking 20 mL of the aqueous suspension of cellulose nanocrystals after sulfuric acid-catalyzed hydrolysis in step S1, taking 1.0-2.5 g of 10% polyvinyl alcohol solution and 0.8 g of MXene suspension and adding them to the aqueous suspension of cellulose nanocrystals, stirring at room temperature for 4 h at 800 rpm in a stirrer to obtain an assembly precursor, and then placing it in a polystyrene culture dish with a diameter of 6 cm, and obtaining a cellulose nanocrystal chiral array co-assembly material by evaporation-induced self-assembly under ambient conditions;

[0070] S4. Preparation of structural color visualization and electrical digital strain sensor materials: The cellulose nanocrystal chiral array co-assembly material prepared in step S3 is soaked in a 3 mol / L NaOH solution at room temperature for 1 hour, and then washed with deionized water until neutral, and finally a bio-based nanoparticle conductive chiral array hydrogel membrane material is obtained;

[0071] S5. Preparation of flexible sensors with structural color visualization and electrical digital strain sensor materials: Cut the bio-based nanoparticle conductive chiral array hydrogel film material prepared in step S4 into strips with a length of 50.0 mm, a width of 10.0 mm, and a thickness of 0.02 mm, and wrap both ends of the strips with copper foil to ensure a close fit with the hydrogel film, then connect the copper foil to a wire and connect it to a multimeter to form a loop to form a flexible sensor.

[0072] Comparative Example 1

[0073] The difference between Comparative Example 1 and Example 1 is that no MXene material is added in step S3.

[0074] Comparative Example 2

[0075] The difference between Comparative Example 2 and Example 2 is that no MXene material is added in step S3.

[0076] Comparative Example 3

[0077] The difference between Comparative Example 3 and Example 3 is that no MXene material is added in step S3.

[0078] Comparative Example 4

[0079] The difference between Comparative Example 4 and Example 4 is that no MXene material is added in step S3.

[0080] Figure 1 This is a cross-sectional scanning electron micrograph of the bio-based nanoparticle conductive chiral array hydrogel film material prepared in step S4 of Example 4, proving that the chiral structure exists in the co-assembled material;

[0081] Figure 2 This is an EDX spectrum diagram of the cross section of the bio-based nanoparticle conductive chiral array hydrogel film material prepared in step S4 of Example 4. Figure 2 The upper left is a scanning electron microscope image of a cross-section of a bio-based nanoparticle conductive chiral array hydrogel film; Figure 2 The upper right shows the distribution of carbon; Figure 2 The lower left is the oxygen element distribution map; Figure 2 The lower right is the distribution diagram of titanium element; it shows that all components are evenly distributed in the material;

[0082] Figure 3The optical photographs of the bio-based nanoparticle conductive chiral array hydrogel film material prepared in step S3 of Example 4 at tensile strains of 40%, 80%, and 120%, respectively, prove that the material has a mechanically stimulated structural color response;

[0083] Figure 4 Comparison of stress-strain curves of bio-based nanoparticle conductive chiral array hydrogel film materials prepared in Examples 1 to 4 with different amounts of polyvinyl alcohol (PVA) added, indicating that as the PVA content increases, the elongation at break and the tensile strength of the material also increase;

[0084] Figure 5 (a) is the correlation between the relative resistance change and tensile strain of the flexible sensor based on the bio-based nanoparticle conductive chiral array hydrogel film material prepared in step S5 of Example 4 of the present invention;

[0085] Figure 5 (b) The relative resistance change of the flexible sensor based on bio-based nanoparticle conductive chiral array hydrogel film material prepared in step S5 of Example 4 after repeated loading and unloading 200 times under 20% tensile strain, demonstrating the good repeatability and durability of the material.

[0086] Figure 6 (a) is the relative resistance change of the flexible sensor based on bio-based nanoparticle conductive chiral array hydrogel film material prepared in step S5 of Example 4 when pressed by a finger.

[0087] Figure 6 (b) is the relative resistance change of the flexible sensor based on bio-based nanoparticle conductive chiral array hydrogel film material prepared in step S5 of Example 4 when smiling.

[0088] Figure 6 (c) is the relative resistance change of the flexible sensor based on bio-based nanoparticle conductive chiral array hydrogel film material prepared in step S5 of Example 4 when making a fist.

[0089] Figure 7 "Hello!" (left) and "Smile" (right) written on a tablet by a simple capacitive pen made of bio-based nanoparticle conductive chiral array hydrogel film material prepared in step S3 of comparative example 4 of the present invention;

[0090] Figure 8 This is a photograph of the bio-based nanoparticle chiral array hydrogel film material after stretching prepared in step S4 of comparative example 4 of the present invention, indicating that the color contrast is not obvious without the addition of MXene;

[0091] Fig. 9These are photos of the cellulose nanocrystal chiral array co-assembly materials prepared in step S3 of Examples 1 to 4 of the present invention. From left to right, the amounts of PVA added are 1.0 g, 1.5 g, 2.0 g, and 2.5 g, respectively, proving that the introduction of MXene does not affect its self-assembly.

[0092] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.

Claims

1. A method for preparing a strain sensing material with structural color visualization and electrical signal digital coupling, characterized in that: The steps include: S1. Preparation of cellulose nanocrystal suspension: treating biomass from different cellulose sources with sulfuric acid to obtain a one-dimensional rod-shaped cellulose nanocrystal (CNC) suspension with high aspect ratio, high specific surface area and excellent photoluminescence performance, and concentrating it to 2-8 wt% by rotary evaporation; S2. Preparation of CNC chiral array and MXene co-assembled material: In order to adjust the proportion of each component in the co-assembled material to adjust the mechanical properties of the material, 10-20% polyvinyl alcohol (PVA) solution, cellulose nanocrystal suspension prepared in step S1 and MXene suspension are mixed in a mass ratio of (10-50):80:(10-15), and magnetically stirred at room temperature for 5 hours to obtain a uniform dispersion; the above dispersion is then placed in an ice water bath and ultrasonically treated with an ultrasonic cleaner for 5-10 minutes to induce the one-dimensional rod-shaped end of the CNC to enter the MXene layer, forming a "needle tip prying" effect, and the cellulose nanocrystal chiral array co-assembled material is obtained by evaporation-induced self-assembly at room temperature. The evaporation-induced self-assembly at room temperature helps to obtain the cellulose nanocrystal chiral array structure of the co-assembled material and take into account the formation of the MXene conductive path; S3. Preparation of structural color visualization and electrical digital strain sensor material: The cellulose nanocrystal chiral array co-assembled material prepared in step S2 is subjected to alkali treatment at room temperature for 1 hour, and then washed with deionized water until neutral to obtain a structural color visualization and electrical digital strain sensor material.

2. The method for preparing the strain sensing material according to claim 1, characterized in that: In step S1, the length of the cellulose nanocrystals ranges from 100 to 700 nm, and the width ranges from 2 to 12 nm; the concentration of the cellulose nanocrystal dispersion is from 0.1 to 1 wt %.

3. The method for preparing the strain sensing material according to claim 1, characterized in that: The specification of the polyvinyl alcohol in step S2 is PVA-1788, and the alcoholysis degree is 87-89.

4. The method for preparing the strain sensing material according to claim 3, characterized in that: In step S2, the ultrasonic power in the ice bath environment is 50-400W, which is conducive to forming a "needle tip prying" effect that induces the one-dimensional rod-shaped end of the CNC to enter the MXene layer, improving the dispersion stability in the MXene suspension, the uniformity of distribution within the material, and the reliability of forming a conductive path.

5. The method for preparing the strain sensing material according to claim 4, characterized in that: The preparation method of the MXene suspension in step S2 is as follows: 1.0-4.0 g of MXene powder is slowly added to a mixed solution containing 20-60 mL of 7-9 mol / L HCl and 3.0-5.0 g of LiF, and then the layered MXene is prepared by continuous stirring at 40°C for 48 h; the resulting solution is then centrifuged and washed three times with 4 mol / L HCl; it is then washed several times with deionized water until the pH of the supernatant is close to neutral; the precipitate obtained by centrifugation is dispersed in a silk-mouth bottle filled with deionized water, and then ultrasonically treated in an ice bath for 1 h; finally, the solution is centrifuged at 5000 rpm for 0.5 h, the upper layer of liquid is collected, and a MXene suspension containing few-layer MXene nanosheets is obtained.

6. The method for preparing the strain sensing material according to claim 5, characterized in that: The solid content of the MXene suspension in step S2 is 0.02-0.1 wt %, which ensures that the MXene forms a conductive pathway and its sensing response is linearly related to the sensitivity and slows down the agglomeration in the CNC / PVA assembly suspension.

7. The method for preparing the strain sensing material according to claim 5, characterized in that: In step S2, the dispersion liquid is heated to 0.05-1.0 mL / (cm 2 ·day) evaporation-induced rate to self-assemble to ensure that the chiral array structure of cellulose nanocrystals and the MXene conductive pathway of the co-assembled material are obtained.

8. A strain sensing material product prepared by the method for preparing a strain sensing material coupling structural color visualization with electrical signal digitization as claimed in any one of claims 1 to 7.

9. Application of the strain sensing material product with structural color visualization and electrical signal digitization coupling as claimed in claim 8 in the fields of visualization and digital intelligent sensing, motion monitoring, and sensing equipment.