Photopolymerization polydiacetylene molecule-based mechanical property enhanced hydrogel and preparation method thereof
By introducing molecules of butadiyne structure into PVA hydrogels and forming polybutadiyne molecules through ultraviolet light irradiation, the problem of poor mechanical properties of PVA hydrogels is solved, and better mechanical properties and optical responsiveness are achieved.
Patent Information
- Application Number
- CN202411156304.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-12-06
AI Technical Summary
Pure PVA hydrogels have poor mechanical properties and elasticity, lack of crosslinking mechanisms and energy loss mechanisms, which limits their application scope.
In PVA, molecules containing butadiene structure, such as 10,12-pendodialylic acid and 10,12-2decadioxylic acid, are introduced, and the crosslinking density is increased through intermolecular forces such as hydrogen bonds, and It is polymerized by ultraviolet light to form polybutadiene molecules, forming a conjugated structure with three bonds and double bonds alternately, enhancing the mechanical properties of the hydrogel.
It significantly improves the mechanical properties and elasticity of the hydrogel, and can generate unique optical signal changes under external stimulation, enhancing its application potential.
Smart Images

Figure CN119081153A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hydrogels, and in particular relates to a mechanical property enhanced hydrogel based on photopolymerized polydiacetylene molecules and a preparation method thereof. Background Art
[0002] Hydrogels are composed of a large amount of water and a three-dimensional polymer network. They have suitable and adjustable mechanical properties and have been widely used in various fields, such as drug delivery, wearable electronic devices, environmental protection, etc. Hydrogels are usually divided into natural hydrogels and synthetic hydrogels. Natural hydrogels are usually prepared from natural polymer materials, such as sodium alginate, chitosan, etc. This type of hydrogel has good biocompatibility, but the strength is usually low, so the application range is narrow. Synthetic hydrogels are usually prepared from synthetic polymer materials, such as polyvinyl alcohol, polyacrylamide, etc. This type of hydrogel can be prepared into a high-strength hydrogel by introducing additional structures and cross-linking mechanisms.
[0003] Polyvinyl alcohol (PVA) is a chemically stable, non-toxic, biocompatible, degradable, and easily processed polymer material, which is widely used in the research and preparation of hydrogels. For pure PVA hydrogels, due to the lack of cross-linking mechanisms and energy loss mechanisms, the mechanical properties and elasticity of PVA hydrogels are poor.
[0004] At present, a variety of methods have been developed to obtain tough and elastic PVA hydrogels. Fang et al. prepared PVA-CBA hydrogels by grafting 4-carboxybenzaldehyde (CBA) onto PVA and then dialyzing it continuously in ethanol and water. The in situ formed dynamic hydrophobic domains solve the contradiction between the high strength and good self-healing ability of hydrogels. Due to the presence of hydrogen bonds, the hydrophobic domains can be reversibly broken and reorganized, allowing the broken hydrogels to quickly and effectively self-heal at room temperature and restore their original mechanical strength. Summary of the invention
[0005] In view of the problems that pure PVA hydrogel has poor performance in the prior art, the present invention provides a mechanical property enhanced hydrogel based on photopolymerized polydiacetylene molecules and a preparation method thereof. The preparation method is to introduce molecules containing diacetylene structures into PVA, such as 10,12-pentacosadiynoic acid (PCDA), 10,12-tricosadiynoic acid (TCDA), etc., and increase the crosslinking density of PVA through intermolecular forces such as hydrogen bonds, so that the prepared hydrogel has good mechanical properties. In addition, since the molecules containing diacetylene structures can respond to ultraviolet light, they can be polymerized to form polydiacetylene molecules (PDA), forming a conjugated structure with alternating triple bonds and double bonds, and further obtaining a new enhanced hydrogel. Since the optical properties of PDA can be changed by external stimuli, the hydrogel obtained by ultraviolet light can produce unique changes in optical signals corresponding to external stimuli.
[0006] The present invention is achieved through the following technical solutions:
[0007] A method for preparing a mechanically enhanced hydrogel based on photopolymerized polydiacetylene molecules, comprising the following steps:
[0008] Step 1: Preparation of vesicles based on molecules containing diacetylene structures;
[0009] The molecules having a diacetylene structure are dissolved in a chloroform solution, the solvent is evaporated using a nitrogen gas flow, deionized water is added, and underwater ultrasound is performed at a certain temperature, and then the solution is kept at a certain temperature for a certain period of time to obtain an aggregate solution based on the molecules containing a diacetylene structure, and then the aggregate solution based on the molecules containing a diacetylene structure is filtered through a 0.45 μm needle filter to remove large particle aggregates to obtain a vesicle solution based on the molecules containing a diacetylene structure;
[0010] Step 2: Preparation of PVA-CBA;
[0011] PVA and CBA were weighed in a certain ratio, added to a solvent to dissolve, then precipitated in ethanol, and finally washed with tetrahydrofuran. After washing, they were placed in a vacuum drying oven for drying to obtain PVA-CBA;
[0012] Step 3: Preparation of PVA-CBA-diacetylene molecular hydrogel;
[0013] The PVA-CBA prepared in step 2 was dissolved in deionized water, and then the vesicle solution based on molecules containing diacetylene structure prepared in step 1 was added to the aqueous solution of PVA-CBA, stirred at room temperature for 5 hours, poured into a polytetrafluoroethylene mold, and finally dried at 40°C for 5-9 days to obtain PVA-CBA-diacetylene molecular hydrogel.
[0014] Furthermore, in step 1, the molecule containing a diacetylene structure is 10,12-pentacosadiynoic acid (PCDA) or 10,12-tricosadiynoic acid (TCDA).
[0015] Furthermore, in step 1, the temperature range of underwater ultrasound is 75° C., and maintained at 4° C. for 12 hours.
[0016] Furthermore, in step 2, the molar ratio of PVA to CBA is 40:1.
[0017] Furthermore, in step 2, the solvent is a mixed solution of dimethyl sulfoxide and hydrochloric acid.
[0018] Furthermore, in step three, the molar ratio of the PVA-CBA to the vesicle solution based on molecules containing a diacetylene structure is 400:1.
[0019] Furthermore, in step three, the PVA-CBA is dissolved by stirring at 85°C.
[0020] Furthermore, the method further comprises:
[0021] The prepared PVA-CBA-diacetylene molecular hydrogel is irradiated with ultraviolet light of 254 nm for a certain period of time to polymerize and form a PVA-CBA-polydiacetylene molecular hydrogel.
[0022] Furthermore, the certain time is 30 minutes.
[0023] Compared with the prior art, the advantages of the present invention are as follows:
[0024] The invention discloses an enhanced PVA hydrogel and a preparation method thereof. Molecules containing a diacetylene structure are introduced into PVA, and the cross-linking density of the PVA is increased by intermolecular forces such as hydrogen bonds, so that the prepared hydrogel has good mechanical properties. Furthermore, since the molecules containing a diacetylene structure can respond to ultraviolet light, they can be polymerized to form PDA, forming a conjugated structure with alternating triple bonds and double bonds, and further obtaining a new enhanced hydrogel. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the following is a brief introduction to the drawings required for the specific embodiments or the description of the prior art. In all the drawings, similar elements or parts are generally identified by similar reference numerals. In the drawings, the elements or parts are not necessarily drawn according to the actual scale.
[0026] Figure 1 It is a schematic diagram of a process for preparing a reinforced PVA hydrogel of the present invention;
[0027] Figure 2 is the particle size distribution diagram of PCDA vesicles;
[0028] Figure 3 is the hydrogen spectrum of PVA-CBA;
[0029] Figure 4 These are the stress-strain curves of PVA-CBA, PVA-CBA-PCDA, and PVA-CBA-PDA hydrogels. DETAILED DESCRIPTION
[0030] In order to clearly and completely describe the technical solution and its specific working process of the present invention, the specific implementation methods of the present invention are as follows in conjunction with the accompanying drawings of the specification:
[0031] Example 1
[0032] like Figure 1 As shown, this embodiment provides a method for preparing an enhanced PVA hydrogel, which specifically includes the following steps:
[0033] Step 1: Preparation of TCDA aggregates;
[0034] 0.0492 g of TCDA was weighed and added to 5 mL of chloroform to dissolve, and the solvent was evaporated using a nitrogen stream. Then 125 mL of water was added, and ultrasonicated at 75° C. for 30 min, and then placed at 4° C. overnight to obtain a TCDA aggregate solution. The TCDA aggregate solution was then filtered through a 0.45 μm needle filter to remove large particle aggregates to obtain a TCDA vesicle solution;
[0035] Step 2: Preparation of PVA-CBA;
[0036] Weigh 2.5 g of PVA, 0.2133 g of CBA, and 1 mL of 1 M hydrochloric acid, dissolve in 20 mL of dimethyl sulfoxide, then precipitate in ethanol, and finally wash with tetrahydrofuran. After washing, put it in a vacuum drying oven and dry it for 24 hours to obtain PVA-CBA;
[0037] Step 3: Preparation of PVA-CBA-TCDA hydrogel;
[0038] The PVA-CBA prepared in step 2 was added to 20 mL of deionized water and stirred to dissolve at 85°C; the TCDA vesicle solution prepared in step 1 was added to the PVA-CBA aqueous solution, stirred at room temperature for 5 h, poured into a polytetrafluoroethylene mold, and finally dried at 40°C for 7 days to obtain PVA-CBA-TCDA hydrogel.
[0039] Step 4: Preparation of PVA-CBA-TCDA hydrogel;
[0040] The prepared PVA-CBA-TCDA hydrogel was irradiated with ultraviolet light at 254 nm for a certain period of time to polymerize and form a PVA-CBA-PDA hydrogel.
[0041] Example 2
[0042] This embodiment provides a method for preparing an enhanced PVA hydrogel, which specifically comprises the following steps:
[0043] Step 1: Preparation of PCDA aggregates;
[0044] 0.0532 g of PCDA was weighed and added to 5 mL of chloroform to dissolve, and the solvent was evaporated using a nitrogen stream, and then 130 mL of water was added, and the mixture was ultrasonicated at 75° C. for 30 min, and then placed at 4° C. overnight to obtain a PCDA aggregate solution, and then the PCDA aggregate solution was filtered through a 0.45 μm needle filter to remove large particle aggregates to obtain a PCDA vesicle solution;
[0045] Step 2: Preparation of PVA-CBA;
[0046] Weigh 2.5 g of PVA, 0.2133 g of CBA, and 1 mL of 1 M hydrochloric acid, dissolve in 20 mL of dimethyl sulfoxide, then precipitate in ethanol, and finally wash with tetrahydrofuran. After washing, put it in a vacuum drying oven and dry it for 24 hours to obtain PVA-CBA;
[0047] Step 3: Preparation of PVA-CBA-PCDA hydrogel;
[0048] The PVA-CBA prepared in step 2 was added to 20 mL of deionized water and stirred at 85°C to dissolve; the PCDA vesicle solution prepared in step 1 was added to the PVA-CBA aqueous solution, stirred at room temperature for 5 h, poured into a polytetrafluoroethylene mold, and finally dried at 40°C for 7 days to obtain a PVA-CBA-PCDA hydrogel;
[0049] Step 4: Preparation of PVA-CBA-PDA hydrogel;
[0050] The PVA-CBA-PCDA hydrogel prepared in step 3 is irradiated with 254 nm ultraviolet light for a certain period of time to polymerize the PCDA monomer molecules to form a PVA-CBA-PDA hydrogel.
[0051] Table 1 is the test performance table
[0052]
[0053] As shown in Table 1, after adding PCDA vesicles, the tensile stress and elastic coefficient of PVA-CBA-PCDA hydrogel were significantly enhanced; through hydrogen bonding, the cross-linking density of PVA-CBA-PCDA hydrogel was increased, thereby enhancing the mechanical properties of PVA-CBA-PCDA hydrogel; when PVA-CBA-PCDA was exposed to ultraviolet light, 1,4-addition reaction occurred between PCDA monomers, and PCDA vesicles were transformed into PDA vesicles, which have a conjugated structure with alternating triple bonds and double bonds. Compared with PCDA vesicles, PDA vesicles have a tougher structure, so PVA-CBA-PDA hydrogel has better mechanical properties.
[0054] like Figure 1 Shown is the preparation process of hydrogel.
[0055] like Figure 2 As shown, the PCDA vesicles were filtered through a 0.45 μm filter, and the particle size distribution after filtration showed that the average particle size of the PCDA vesicles was about 200 nm.
[0056] like Figure 3 As shown, hydrogen spectrum characterization showed that the CBA group was successfully connected to the PVA molecule.
[0057] like Figure 4 As shown, tensile tests were carried out on the prepared hydrogel materials. After the addition of PCDA vesicles, the mechanical properties of the hydrogel were significantly improved. After the PCDA vesicles were polymerized under ultraviolet light, the hydrogel had better mechanical properties.
[0058] The preferred embodiments of the present invention are described in detail above in conjunction with the accompanying drawings. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0059] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0060] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for preparing a mechanically enhanced hydrogel based on photopolymerized polydiacetylene molecules, comprising the following steps: Step 1: Preparation of vesicles based on molecules containing diacetylene structures; The molecule having a diacetylene structure is dissolved in a chloroform solution, the solvent is evaporated by a nitrogen gas flow, deionized water is added, and underwater ultrasound is performed at a certain temperature, and then the solution is kept at a certain temperature for a certain period of time to obtain an aggregate solution based on the molecule containing a diacetylene structure, and then the aggregate solution based on the molecule containing a diacetylene structure is filtered through a 0.45 μm needle filter to remove large particle aggregates to obtain a vesicle solution based on the molecule containing a diacetylene structure; Step 2: Preparation of PVA-CBA; PVA and CBA were weighed in a certain ratio, added to a solvent to dissolve, then precipitated in ethanol, and finally washed with tetrahydrofuran. After washing, they were placed in a vacuum drying oven for drying to obtain PVA-CBA; Step 3: Preparation of PVA-CBA-diacetylene molecular hydrogel; The PVA-CBA prepared in step 2 was dissolved in deionized water, and then the vesicle solution based on molecules containing diacetylene structure prepared in step 1 was added to the aqueous solution of PVA-CBA, stirred at room temperature for 5 hours, poured into a polytetrafluoroethylene mold, and finally dried at 40°C for 5-9 days to obtain PVA-CBA-diacetylene molecular hydrogel.
2. The method for preparing a mechanically enhanced hydrogel based on photopolymerized polydiacetylene molecules according to claim 1, characterized in that: In step 1, the molecule containing a diacetylene structure is 10,12-pentacosadiynoic acid or 10,12-tricosadiynoic acid.
3. The method for preparing a mechanically enhanced hydrogel based on photopolymerized polydiacetylene molecules according to claim 1, characterized in that: In step 1, the temperature range of underwater ultrasound is 75°C and maintained at 4°C for 12 hours.
4. The method for preparing a mechanically enhanced hydrogel based on photopolymerized polydiacetylene molecules according to claim 1, characterized in that: In step 2, the molar ratio of PVA to CBA is 40:
1.
5. The method for preparing a mechanically enhanced hydrogel based on photopolymerized polydiacetylene molecules according to claim 1, characterized in that: In step 2, the solvent is a mixed solution of dimethyl sulfoxide and hydrochloric acid.
6. The method for preparing a mechanically enhanced hydrogel based on photopolymerized polydiacetylene molecules according to claim 1, characterized in that: In step 2, the molar ratio of the PVA-CBA to the vesicle solution based on molecules containing a diacetylene structure is 400:
1.
7. The method for preparing a mechanically enhanced hydrogel based on photopolymerized polydiacetylene molecules according to claim 1, characterized in that: The PVA-CBA was dissolved under stirring at 85°C.
8. The method for preparing a mechanically enhanced hydrogel based on photopolymerized polydiacetylene molecules according to claim 1, characterized in that: The method further comprises: The prepared PVA-CBA-diacetylene molecular hydrogel is irradiated with ultraviolet light of 254 nm for a certain period of time to polymerize and form a PVA-CBA-polydiacetylene molecular hydrogel.
9. The method for preparing a mechanically enhanced hydrogel based on photopolymerized polydiacetylene molecules according to claim 1, characterized in that: The certain period of time is 30 minutes.