Method for manufacturing white solar backboard base film through direct melting method
The fluorine-free white solar backplane base film is manufactured through direct melting method, and the fluorine pollution problem is solved by using dicarboxylic acids, alcohols and inorganic particle additives, and the preparation of high-performance base film is achieved, extending service life and reducing production costs .
Patent Information
- Application Number
- CN202311317926.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-08-30
- Filing Date
- 2023-10-12
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-10-12
AI Technical Summary
The existing solar back panel base film contains fluorine compounds, which leads to fluorine pollution problems. It is necessary to develop alternatives that do not contain fluorine to reduce environmental pollution.
The direct melting method is used to manufacture the white solar back panel base film, and the dicarboxylic acid, alcohol and inorganic particle additives are used to form a non-existent carboxylic acid, alcohol and inorganic particle additives through the steps of slurry, catalyst liquid, ester compound, additive melt, pre-polycondensation and final polycondensation. High-performance base film of fluorine.
A white solar backplane base film without fluorine was prepared, which has excellent photoaging resistance, hydrolysis resistance and water vapor barrier properties, extends service life, reduces production costs, and reduces fluorine pollution.
Smart Images

Figure BDA0004489969590000131 
Figure BDA0004489969590000141 
Figure BDA0004489969590000151
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solar energy, and in particular to a method for manufacturing a white solar backplane base film by a direct melting method. Background Art
[0002] The solar backsheet base film is a polymer base film attached to the solar backsheet, and its purpose is to improve the stability of the working performance and service life of the solar panel. When in use, you only need to press the solar backsheet base film on the solar backsheet, and the base film can be firmly adsorbed on the solar backsheet through the interaction of van der Waltz forces.
[0003] In the related art, there are two main types of solar backplane base films: one is a coated backplane base film, which is made by coating a fluorine-containing resin on the surface of the base material PET polyester film; the other is a glue-coated composite backplane base film, which is made by composite a fluorine film on the surface of the base material PET polyester film. The function of the fluorine-containing resin layer or the fluorine film is to form a protective film on the surface of the solar backplane, making the solar backplane more durable, light-resistant, heat-resistant and corrosion-resistant, and extending the service life of the solar backplane.
[0004] However, since the above two types of solar backplane base films both contain fluorine, and fluorine pollution caused by fluorine compounds is an environmental problem that the entire society is currently facing, it is necessary to develop a fluorine-free solar backplane base film to reduce fluorine pollution. Summary of the invention
[0005] In order to reduce fluorine pollution caused by manufacturing a solar backplane base film, the present application provides a method for manufacturing a white solar backplane base film by a direct melting method.
[0006] In a first aspect, the present application provides a method for manufacturing a white solar backplane base film by a direct melting method, using the following technical solution: A method for manufacturing a white solar backplane base film by a direct melting method comprises the following steps: Slurry preparation: mixing one of the dicarboxylic acid or the dimethyl dicarboxylate with the diol to obtain a slurry; Preparation of catalyst liquid: dissolving the catalyst in diol to obtain catalyst liquid; Preparation of esterification product: Mix the slurry and the catalyst solution, heat to 160-265°C and react for 4-5 hours to obtain the esterification product; Preparation of additive melt: melt-blending the inorganic particle additive and the polyester chips at 260-280° C. to obtain the additive melt; Pre-condensation: The esterification product and the additive melt are mixed, and a pre-condensation reaction is carried out in a vacuum environment at 200-280°C, and then the excess diol is discharged to obtain a pre-condensation product; Final polycondensation: subjecting the pre-polycondensation product to a polycondensation reaction in a vacuum environment at 280-285°C to obtain a final polycondensation product; Molding: The final polycondensation product is pumped into the die head, and after sheet casting, cooling molding, longitudinal stretching, transverse stretching, heat setting and corona treatment, a white solar backplane base film is obtained.
[0007] By adopting the above technical scheme, the present application obtains a slurry with a diol as the matrix through the slurry preparation step, and obtains a catalyst liquid with a diol as the matrix through the catalyst liquid preparation step, which helps to improve the compatibility of the slurry and the catalyst liquid in the esterification preparation step, and facilitates the catalytic reaction. Moreover, before the pre-polycondensation step and the final polycondensation step, the inorganic particle additive and the polyester chips are made into an additive melt. By pre-forming the additive melt, the inorganic particle additive is not only fully dispersed before being added to the reactor, but also avoids the large amount of ethylene glycol solution consumed by the solvent method for preparing the inorganic particle additive and the temperature fluctuation and energy loss caused by the addition of a large amount of ethylene glycol to the reactor, and can obtain a final polycondensation product with the inorganic particle additive uniformly dispersed inside. A white solar back panel base film can be prepared using this final polycondensation product. The white solar back panel base film has excellent light aging resistance, hydrolysis resistance and water vapor barrier properties. The white solar back panel base film can be used on the solar back panel, which can also meet the service life requirements of the solar back panel, help reduce the cost of manufacturing the solar back panel, and the fluorine pollution that may be caused after the solar back panel is scrapped.
[0008] In a specific embodiment, in the slurry step, when a dicarboxylic acid is mixed with a diol, the molar ratio of the dicarboxylic acid to the diol is 1:1.15-1:1.7, and when a dimethyl dicarboxylate is mixed with a diol, the molar ratio of the dimethyl dicarboxylate to the diol is 1:1.8-1:2.4; the dicarboxylic acid includes at least one of terephthalic acid and isophthalic acid, the dimethyl dicarboxylate includes at least one of ethylene terephthalate, ethylene isophthalate and ethylene naphthalate, and the diol includes at least one of ethylene glycol, neopentyl glycol, propylene glycol, butanediol and 1,4-cyclohexanedimethanol.
[0009] By adopting the above technical solution, there is a reaction difference between dicarboxylic acid and dimethyl dicarboxylate in the process of reacting with diol, therefore, it is necessary to control the amount of dicarboxylic acid and dimethyl dicarboxylate. The present application has found through experiments that when the above specific components are selected, the molar ratio of dicarboxylic acid to diol or the molar ratio of dimethyl dicarboxylate to diol is controlled within the above range, and the prepared slurry can undergo a good esterification reaction with the catalyst liquid, and the obtained white solar backplane base film has higher tensile strength and elongation at break, and lower thermal shrinkage, which shows that within the above molar ratio range, the durability and heat resistance of the base film can be improved, which helps to extend the service life of the base film.
[0010] In a specific embodiment, in the step of preparing the catalyst liquid, the diol is ethylene glycol, and the diol and the catalyst are mixed in a weight ratio of 100:(1-3), and dissolved at 175-188°C to obtain a catalyst liquid; when a dicarboxylic acid is mixed with a diol, the catalyst is antimony trioxide; when a dimethyl dicarboxylate is mixed with a diol, the catalyst is a mixture of one or more of calcium acetate, cadmium acetate, zinc acetate, magnesium acetate, and cobalt acetate.
[0011] By adopting the above technical solution, when the above components are used to prepare the catalyst liquid, at the above temperature, ethylene glycol and antimony trioxide can react to form ethylene glycol antimony, and by adopting the above weight ratio, a catalyst liquid with a catalyst mass concentration of 1-5% can be prepared. The present application has found through experiments that the use of this catalyst liquid can react well with the above slurry, and the prepared base film has a significantly lower water vapor permeability than the base film coated with fluorine-containing resin or covered with fluorine film, and the total irradiation of the high pressure cooking test for 72 hours and the UV test reaches 180kwh / m 2 After the film is coated with water, it still has a high elongation at break, which shows that the use of the above specific component ratio is helpful to improve the high temperature and high pressure resistance and light aging resistance of the base film.
[0012] In a specific embodiment, in the esterification preparation step, the slurry and the catalyst liquid are mixed in a weight ratio of (87.5-98):(2-12.5).
[0013] An ester with an ethylene glycol antimony content of 400-500 ppm can be prepared. The present application has found through experiments that maintaining the above range helps to improve the tensile properties and elongation at break of the base film and reduce the thermal shrinkage.
[0014] In a specific embodiment, in the step of preparing the additive melt, the particle size of the inorganic particle additive is 0.1-0.7 μm, the weight ratio of the inorganic particle additive to the polyester chip is (4-50):100, and the inorganic particle additive includes at least one of mica, barium sulfate, kaolin, titanium dioxide, calcium carbonate, silicon dioxide, talc and montmorillonite.
[0015] By adopting the above technical solution, when the particle size of the inorganic particle additive is too small, the dispersibility of the inorganic particle additive in the melt is poor, and when the particle size of the inorganic particle additive is large, it will affect the light transmittance and surface smoothness of the base film. By adopting the inorganic particle additive with the above particle size and specific composition and the above weight ratio, the dispersibility of the inorganic particle additive in the melt can be improved, and the light transmittance of the base film can be controlled within the desired range, thereby improving the light diffusion and light aging resistance of the base film, and also improving the tensile strength and heat resistance of the base film.
[0016] In a specific possible implementation scheme, in the pre-condensation step, the esterified product and the additive melt are mixed to obtain a mixture, the mass fraction of the additive melt in the mixture is 10%-30%, and the pre-condensation reaction is carried out at a vacuum degree of 1-10KPa and a temperature of 270-280°C for 2-3h, and then the excess diol is discharged to obtain a pre-condensation product.
[0017] By adopting the above technical scheme, the mass fraction of the additive melt is controlled within the above range, and the reaction conditions are controlled within the above range, which helps to improve the yield of the precondensation polymer. Moreover, the polymerization degree of the precondensation polymer can be controlled within a more appropriate range, thereby improving the fluidity of the precondensation polymer and facilitating the transportation of the precondensation polymer.
[0018] In a specific embodiment, in the final polycondensation step, the pre-polycondensation product is subjected to a polycondensation reaction at a vacuum degree of 100-200 Pa and a temperature of 280-285° C. for 2-3 hours to obtain a final polycondensation product.
[0019] By adopting the above technical scheme, when the precondensate is prepared by the above process conditions, the process conditions of the final polycondensation step are controlled within the above range, and a final polycondensation product can be obtained. The final polycondensation product not only has excellent fluidity and is easy to transport, but also has high tensile strength and elongation at break, low heat shrinkage, low light transmittance and water vapor permeability, good light dispersion, and excellent high temperature and high pressure resistance and light aging resistance.
[0020] In a specific possible implementation method, the final polycondensation step further includes the following steps: mixing the final polycondensation product with an online viscosity enhancer until uniform to obtain a final polycondensation melt, the quality indicators of the final polycondensation melt are as follows: intrinsic viscosity 0.80dl / g-0.90dl / g, terminal carboxyl group ≤20mmol / t, melting point 250°C-272°C, ash content ≤0.06%; in the molding step, the final polycondensation melt is pumped into the die head.
[0021] By adopting the above technical scheme, due to the addition of a large amount of inorganic particle additives, the dynamic viscosity of the melt is relatively large. During the melt conveying process, the pressure drop is very large and it is not easy to convey. Therefore, it is not suitable to add a tackifier during the pre-polycondensation reaction and the final polycondensation reaction. Therefore, the present application adopts an online tackification process. After the final polycondensation product is prepared, the final polycondensation product is mixed with the online tackifier added online, so that the melt viscosity is rapidly improved, and finally the final polycondensation melt that meets the high viscosity requirements of the backplane base film for the melt is obtained. Therefore, the above process is adopted, which is not only convenient for conveying materials, but also can adjust the final polycondensation melt to the required viscosity, so as to obtain the required base film.
[0022] In a specific embodiment, the mass fraction of the online viscosity enhancer in the final polycondensation melt is 0.2%-3.0%, and the online viscosity enhancer includes any one of oxazoline, isocyanate, pyromellitic anhydride, trimellitic anhydride, and glycidyl ether epoxy compounds.
[0023] By adopting the above technical scheme, the present applicant has found through experiments that when the above specific compounds are used as online thickeners and the mass fraction of the online thickeners is controlled within the above range, the tensile strength of the finally prepared base film is further increased, the heat shrinkage rate and water vapor permeability are further reduced, and the high temperature and high pressure resistance is better.
[0024] In a second aspect, the present application provides a white solar backplane base film, which adopts the following technical solution: A white solar back panel base film, characterized in that it is made by the above-mentioned direct melting method for manufacturing white solar back panel base film.
[0025] In summary, the present application includes at least one of the following beneficial technical effects: 1. The method of the present application can prepare a fluorine-free white solar backsheet base film, and the white solar backsheet base film has excellent light aging resistance, hydrolysis resistance and water vapor barrier properties, which helps to reduce the cost of manufacturing solar backsheets and the fluorine pollution that may be caused after the solar backsheets are scrapped; 2. The method of the present application can further improve the light aging resistance, hydrolysis resistance and water vapor barrier performance of the base film by optimizing the process conditions and raw material ratio; 3. The method of the present application can reduce the brittleness or warping of the base film and reduce the occurrence of stretching spots during the stretching process of the base film. DETAILED DESCRIPTION
[0026] Unless otherwise specified, the raw materials used in the examples and comparative examples of the present application were commercially available.
[0027] The present application is further described in detail below in conjunction with embodiments and comparative examples. Example
[0028] Example 1 This embodiment provides a method for manufacturing a white solar backplane base film by a direct melting method, which adopts the following steps: The slurry is prepared by the following operation: terephthalic acid and ethylene glycol are added into a pulping kettle at a weight ratio of 1:1.42, and stirred and pulped until uniform to obtain a slurry.
[0029] The catalyst liquid is prepared by the following operation: ethylene glycol and antimony trioxide are added into a preparation kettle at a weight ratio of 50:1, stirred until uniform, and the temperature in the preparation kettle is heated to 182° C. to react to obtain the catalyst liquid.
[0030] The esterification product is prepared as follows: the slurry and the catalyst liquid are added into the esterification kettle at a weight ratio of 92.3:7.2, stirred until uniform, the temperature in the esterification kettle is heated to 205° C. and then the reaction is carried out at a constant temperature for 4.5 hours, and the heating is stopped to obtain the esterification product.
[0031] The additive melt is prepared by the following operation: adding mica particles with a particle size of 0.1-0.7 μm and PET chips in a weight ratio of 27:100 into a screw extruder, melting and blending at a temperature range of 260-280° C. to obtain the additive melt.
[0032] The pre-condensation reaction is carried out as follows: the esterification product and the additive melt are introduced into the pre-condensation kettle at a mass ratio of 4:1, and mixed until uniform to obtain a mixture, in which the mass fraction of the additive melt in the mixture is 20%, and then the pre-condensation kettle is evacuated and heated, and the reaction environment in the pre-condensation kettle is maintained within the range of a vacuum degree of 6±1 KPa and a temperature of 240±1°C. After the pre-condensation reaction is carried out for 2.5 hours, the reaction is stopped, and the excess diol in the pre-condensation kettle is discharged to obtain a pre-condensation product.
[0033] The final polycondensation reaction is carried out as follows: the pre-polycondensation product is introduced into the final polycondensation kettle, the final polycondensation kettle is evacuated, and the final polycondensation kettle is heated. The reaction environment in the final polycondensation kettle is maintained within the range of a vacuum degree of 150±1Pa and a temperature of 283±1°C, and the polycondensation reaction is carried out for 2.5 hours, and then the reaction is stopped to obtain a final polycondensation product.
[0034] The molding operation is as follows: the final polycondensation product is pumped into the die head, and then the final polycondensation product is cast through the die head onto a cooling roller at 22.5°C to obtain a cast sheet. At the same time, a leeward device is used to blow air on the side of the cast sheet away from the cooling roller. The blowing temperature is 17.5°C and the wind speed is 12.5m / s. After cooling and molding, the cast sheet is sent to a longitudinal stretching machine, the cast sheet is first preheated at 80°C, and then the temperature of the cast sheet is heated to 100°C by infrared heating, and then 3.3 times longitudinal stretching is performed. After the longitudinal stretching is completed, it is cooled and shaped at 23°C to obtain a longitudinal drawn sheet, and then the longitudinal drawn sheet is placed in an oven, preheated at 100°C, and then placed in a transverse stretching machine, and 3.4 times transverse stretching is performed at 115°C after the transverse stretching is completed. A transverse sheet is obtained, the transverse sheet is subjected to high-temperature shaping treatment at 215°C, and then cooled and trimmed at 105°C, and finally rolled up after corona treatment to obtain a white solar backplane base film.
[0035] Example 2 This embodiment provides a method for manufacturing a white solar backplane base film by a direct melting method, which is different from Embodiment 1 only in that an equal amount of isophthalic acid is used to replace terephthalic acid.
[0036] Example 3 This embodiment provides a method for manufacturing a white solar backplane base film by a direct melting method, which is different from Embodiment 1 only in that an equal amount of neopentyl glycol is used to replace ethylene glycol.
[0037] Example 4 This embodiment provides a method for manufacturing a white solar backplane base film by a direct melting method, which is different from Embodiment 1 only in that terephthalic acid and ethylene glycol are added to a pulping kettle at a weight ratio of 1:1.15, stirred and pulped until uniform, to obtain a slurry.
[0038] Example 5 This embodiment provides a method for manufacturing a white solar backplane base film by a direct melting method, which is different from Embodiment 1 only in that terephthalic acid and ethylene glycol are added to a pulping kettle at a weight ratio of 1:1.7, stirred and pulped until uniform, to obtain a slurry.
[0039] Example 6 This embodiment provides a method for manufacturing a white solar backplane base film by a direct melting method. The only difference from Embodiment 1 is that a slurry is prepared first. The operation is as follows: ethylene terephthalate and ethylene glycol are added into a pulping kettle at a weight ratio of 1:2.1, stirred and pulped until uniform, to obtain a slurry.
[0040] Example 7 This embodiment provides a method for manufacturing a white solar backplane base film by a direct melting method, which is different from Embodiment 6 only in that ethylene terephthalate and ethylene glycol are added to a pulping kettle at a weight ratio of 1:1.8, stirred and pulped until uniform, to obtain a slurry.
[0041] Example 8 This embodiment provides a method for manufacturing a white solar backplane base film by a direct melting method, which is different from Embodiment 6 only in that ethylene terephthalate and ethylene glycol are added to a pulping kettle at a weight ratio of 1:2.4, stirred and pulped until uniform, to obtain a slurry.
[0042] Example 9 This embodiment provides a method for manufacturing a white solar backplane base film by a direct melting method, which is different from Embodiment 6 only in that an equal amount of ethylene isophthalate is used to replace ethylene terephthalate.
[0043] Example 10 This embodiment provides a method for manufacturing a white solar backplane base film by a direct melting method. The only difference from Example 1 is that ethylene glycol and antimony trioxide are added to a preparation kettle at a weight ratio of 100:1, stirred until uniform, and the temperature in the preparation kettle is heated to 188°C for reaction to obtain a catalyst liquid.
[0044] Embodiment 11 This embodiment provides a method for manufacturing a white solar backplane base film by a direct melting method. The only difference from Example 1 is that ethylene glycol and antimony trioxide are added to a preparation kettle at a weight ratio of 100:3, stirred until uniform, and the temperature in the preparation kettle is heated to 175°C for reaction to obtain a catalyst liquid.
[0045] Example 12 This embodiment provides a method for manufacturing a white solar backplane base film by a direct melting method. The only difference from Example 1 is that ethylene glycol and antimony trioxide are added to a preparation kettle at a weight ratio of 110:1, stirred until uniform, and the temperature in the preparation kettle is heated to 190°C for reaction to obtain a catalyst liquid.
[0046] Embodiment 13 This embodiment provides a method for manufacturing a white solar backplane base film by a direct melting method. The only difference from Example 1 is that ethylene glycol and antimony trioxide are added to a preparation kettle at a weight ratio of 100:4, stirred until uniform, and the temperature in the preparation kettle is heated to 173°C for reaction to obtain a catalyst liquid.
[0047] Embodiment 14 The present embodiment provides a method for manufacturing a white solar backplane base film by a direct melting method, which is different from the first embodiment in that the slurry and the catalyst liquid are added to the esterification kettle at a weight ratio of 87.5:12.5, stirred until uniform, the temperature in the esterification kettle is heated to 205°C, and the reaction is carried out at a constant temperature for 4.5 hours, and the heating is stopped to obtain an esterified product.
[0048] Embodiment 15 The present embodiment provides a method for manufacturing a white solar backplane base film by a direct melting method, which is different from the first embodiment only in that the slurry and the catalyst liquid are added to the esterification kettle at a weight ratio of 98:2, stirred until uniform, the temperature in the esterification kettle is heated to 205°C and then the reaction is carried out at a constant temperature for 4.5 hours, and the heating is stopped to obtain an esterified product.
[0049] Example 16 The present embodiment provides a method for manufacturing a white solar backplane base film by a direct melting method, which is different from the embodiment 1 only in that the slurry and the catalyst liquid are added to the esterification kettle in a weight ratio of 92.3:7.2, stirred until uniform, the temperature in the esterification kettle is heated to 160°C and then the reaction is carried out at a constant temperature for 5 hours, and the heating is stopped to obtain an esterified product.
[0050] Embodiment 17 The present embodiment provides a method for manufacturing a white solar backplane base film by a direct melting method, which is different from the first embodiment in that the slurry and the catalyst liquid are added to the esterification kettle in a weight ratio of 92.3:7.2, stirred until uniform, the temperature in the esterification kettle is heated to 265°C and then the reaction is carried out at a constant temperature for 4 hours, and the heating is stopped to obtain an esterified product.
[0051] Embodiment 18 This embodiment provides a method for manufacturing a white solar backplane base film by a direct melt method. The only difference from Example 1 is that mica particles with a particle size of 0.1-0.7 μm and PET chips are added to a screw extruder at a weight ratio of 1:25, and melted and blended in a temperature range of 260-280°C to obtain an additive melt.
[0052] Embodiment 19 This embodiment provides a method for manufacturing a white solar backplane base film by a direct melt method. The only difference from Example 1 is that mica particles with a particle size of 0.1-0.7 μm and PET chips are added to a screw extruder in a weight ratio of 1:2, and melted and blended in a temperature range of 260-280°C to obtain an additive melt.
[0053] Embodiment 20 This embodiment provides a method for manufacturing a white solar backplane base film by a direct melt method. The only difference from Example 1 is that mica particles with a particle size of 0.05-0.1 μm and PET chips are added to a screw extruder at a weight ratio of 1:23, and melted and blended in a temperature range of 260-280°C to obtain an additive melt.
[0054] Embodiment 21 This embodiment provides a method for manufacturing a white solar backplane base film by a direct melt method. The only difference from Example 1 is that mica particles with a particle size of 0.7-1 μm and PET chips are added to a screw extruder at a weight ratio of 1:1.8, and melted and blended in a temperature range of 260-280°C to obtain an additive melt.
[0055] Embodiment 22 This embodiment provides a method for manufacturing a white solar backplane base film by a direct melting method, which is different from Embodiment 1 only in that an equal amount of barium sulfate particles are used to replace mica particles.
[0056] Embodiment 23 The present embodiment provides a method for manufacturing a white solar backplane base film by a direct melting method, which is different from Embodiment 1 only in that the esterification product and the additive melt are introduced into a precondensation kettle at a mass ratio of 9:1 and mixed until uniform to obtain a mixture, wherein the mass fraction of the additive melt in the mixture is 10%, and then the precondensation kettle is evacuated and heated, and the reaction environment in the precondensation kettle is maintained within the range of a vacuum degree of 1±1 KPa and a temperature of 200±1°C. After the precondensation reaction is carried out for 3 hours, the reaction is stopped, and the excess diol in the precondensation kettle is discharged to obtain a precondensation product.
[0057] Embodiment 24 The present embodiment provides a method for manufacturing a white solar backplane base film by a direct melting method, which is different from Embodiment 1 only in that the esterification product and the additive melt are introduced into a precondensation kettle in a mass ratio of 7:3 and mixed until uniform to obtain a mixture, in which the mass fraction of the additive melt in the mixture is 30%, and then the precondensation kettle is evacuated and heated, and the reaction environment in the precondensation kettle is maintained within the range of a vacuum degree of 10±1 KPa and a temperature of 280±1°C. After the precondensation reaction is carried out for 2 hours, the reaction is stopped, and the excess diol in the precondensation kettle is discharged to obtain a precondensation product.
[0058] Embodiment 25 The present embodiment provides a method for manufacturing a white solar backplane base film by a direct melting method, which is different from Embodiment 1 only in that the esterification product and the additive melt are introduced into a precondensation kettle in a mass ratio of 6:4 and mixed until uniform to obtain a mixture, in which the mass fraction of the additive melt in the mixture is 40%, and then the precondensation kettle is evacuated and heated, and the reaction environment in the precondensation kettle is maintained within the range of a vacuum degree of 12±1 KPa and a temperature of 290±1°C. After the precondensation reaction is carried out for 1.5 hours, the reaction is stopped, and the excess diol in the precondensation kettle is discharged to obtain a precondensation product.
[0059] Embodiment 26 The present embodiment provides a method for manufacturing a white solar backplane base film by a direct melting method, which is different from Embodiment 1 only in that the esterification product and the additive melt are introduced into a precondensation kettle at a mass ratio of 9.5:0.5, and mixed until uniform to obtain a mixture, in which the mass fraction of the additive melt in the mixture is 5%, and then the precondensation kettle is evacuated and heated, and the reaction environment in the precondensation kettle is maintained within the range of a vacuum degree of 0.5±1KPa and a temperature of 190±1°C. After the precondensation reaction is carried out for 3.5 hours, the reaction is stopped, and the excess diol in the precondensation kettle is discharged to obtain a precondensation product.
[0060] Embodiment 27 The present embodiment provides a method for manufacturing a white solar backplane base film by a direct melting method, which is different from Embodiment 1 only in that the pre-condensation product is introduced into a final condensation kettle, the final condensation kettle is evacuated, and the final condensation kettle is heated. The reaction environment in the final condensation kettle is maintained within the range of a vacuum degree of 100±1Pa and a temperature of 280±1°C. After the condensation reaction is carried out for 3 hours, the reaction is stopped to obtain a final condensation product.
[0061] Embodiment 28 The present embodiment provides a method for manufacturing a white solar backplane base film by a direct melt process, which is different from Embodiment 1 only in that the pre-condensation product is introduced into a final condensation kettle, the final condensation kettle is evacuated, and the final condensation kettle is heated. The reaction environment in the final condensation kettle is maintained within the range of a vacuum degree of 200±1Pa and a temperature of 285±1°C. After the condensation reaction is carried out for 2 hours, the reaction is stopped to obtain a final condensation product.
[0062] Embodiment 29 The present embodiment provides a method for manufacturing a white solar backplane base film by a direct melting method, which is different from Embodiment 1 only in that the pre-condensation product is introduced into a final condensation kettle, the final condensation kettle is evacuated, and the final condensation kettle is heated. The reaction environment in the final condensation kettle is maintained within the range of a vacuum degree of 90±1Pa and a temperature of 278±1°C, and the condensation reaction is carried out for 3.3 hours, and then the reaction is stopped to obtain a final condensation product.
[0063] Embodiment 30 The present embodiment provides a method for manufacturing a white solar backplane base film by a direct melting method, which is different from Embodiment 1 only in that the pre-condensation product is introduced into a final condensation kettle, the final condensation kettle is evacuated, and the final condensation kettle is heated. The reaction environment in the final condensation kettle is maintained within the range of a vacuum degree of 210±1Pa and a temperature of 287±1°C, and the condensation reaction is carried out for 1.8 hours, and then the reaction is stopped to obtain a final condensation product.
[0064] Embodiment 31 The present embodiment provides a method for manufacturing a white solar backplane base film by a direct melting method, which is different from the embodiment 1 only in that the pre-condensation product is introduced into a final condensation kettle, the final condensation kettle is evacuated, and the final condensation kettle is heated, and the reaction environment in the final condensation kettle is maintained within the range of a vacuum degree of 150±1Pa and a temperature of 283±1°C for 2.5 hours of condensation reaction, and then the reaction is stopped to obtain a final condensation product, and then the final condensation product is guided out of the final condensation kettle. In the process of conveying the final condensation product, oxazoline is added to the final condensation product, and the weight ratio of oxazoline to the final condensation product is 1.5:98.5. After uniform mixing, a final condensation melt is obtained.
[0065] Embodiment 32 This embodiment provides a method for manufacturing a white solar backplane base film by a direct melting method. The only difference from Example 31 is that during the process of conveying the final polycondensation product, oxazoline is added to the final polycondensation product. The weight ratio of oxazoline to the final polycondensation product is 0.2:99.8. After uniform mixing, a final polycondensation melt is obtained.
[0066] Embodiment 33 This embodiment provides a method for manufacturing a white solar backplane base film by a direct melting method. The only difference from Example 31 is that during the process of conveying the final polycondensation product, oxazoline is added to the final polycondensation product. The weight ratio of oxazoline to the final polycondensation product is 3:97. After uniform mixing, a final polycondensation melt is obtained.
[0067] Embodiment 34 This embodiment provides a method for manufacturing a white solar backplane base film by a direct melt process, which is different from Example 31 only in that an equal amount of isocyanate is used to replace oxazoline.
[0068] Embodiment 35 The present embodiment provides a method for manufacturing a white solar backplane base film by a direct melt process, which is different from the embodiment 1 only in that the final polycondensation product is pumped into a die head, and then the final polycondensation product is cast through the die head onto a cooling roller at 15°C to obtain a cast sheet. At the same time, a leeward device is used to blow air on the side of the cast sheet away from the cooling roller, and the blowing temperature is 5°C and the wind speed is 5m / s. After cooling and forming, the cast sheet is sent to a longitudinal stretching machine, the cast sheet is first preheated at 70°C, and then the temperature of the cast sheet is heated to 90°C by infrared heating, and then 2.6 times longitudinal stretching is performed. After the longitudinal stretching is completed, it is cooled and shaped at 15°C to obtain a longitudinal drawn sheet, and then the longitudinal drawn sheet is placed in an oven, preheated at 80°C, and then placed in a transverse stretching machine, and 2.8 times transverse stretching is performed at 90°C. After the transverse stretching is completed, a transverse sheet is obtained, the transverse sheet is subjected to high-temperature shaping treatment at 180°C, and then cooled and trimmed at 30°C, and finally rolled up after corona treatment to obtain a white solar backplane base film.
[0069] Embodiment 36 This embodiment provides a method for manufacturing a white solar backplane base film by a direct melting method. The only difference from the first embodiment is that the final polycondensation product is pumped into a die head, and then the final polycondensation product is cast through the die head onto a cooling roller at 30°C to obtain a casting sheet. At the same time, a leeward device is used to blow air to the side of the casting sheet away from the cooling roller. The blowing temperature is 30°C and the wind speed is 20m / s. After cooling and forming, the casting sheet is sent to a longitudinal stretching machine, and the casting sheet is first preheated at 90°C, and then the casting sheet is heated by infrared heating. The temperature is heated to 110°C, and then 4.0 times longitudinal stretching is carried out. After the longitudinal stretching is completed, it is cooled and shaped at 30°C to obtain a longitudinal pulled sheet. The longitudinal pulled sheet is then placed in an oven and preheated at 120°C. The longitudinal pulled sheet is then placed in a transverse stretching machine and 4.0 times transverse stretching is carried out at 140°C. After the transverse stretching is completed, a transverse sheet is obtained. The transverse sheet is subjected to high-temperature shaping treatment at 250°C, and then cooled and trimmed at 180°C. Finally, it is rolled up after corona treatment to obtain a white solar backplane base film.
[0070] Comparative Example Comparative Example 1 This comparative example provides a method for manufacturing a solar backsheet base film, using the following steps: The esterification product is prepared as follows: terephthalic acid, ethylene glycol and antimony trioxide are added into an esterification kettle in a weight ratio of 38.14:62.22:0.14, and stirred until uniform. The temperature in the esterification kettle is heated to 205° C. and the reaction is carried out at a constant temperature for 4.5 hours. The heating is stopped to obtain the esterification product.
[0071] The additive melt is prepared by the following operation: adding mica particles with a particle size of 0.1-0.7 μm and PET chips in a weight ratio of 27:100 into a screw extruder, melting and blending at a temperature range of 260-280° C. to obtain the additive melt.
[0072] The pre-condensation reaction is carried out as follows: the esterification product and the additive melt are introduced into the pre-condensation kettle at a mass ratio of 4:1, and mixed until uniform to obtain a mixture, in which the mass fraction of the additive melt in the mixture is 20%, and then the pre-condensation kettle is evacuated and heated, and the reaction environment in the pre-condensation kettle is maintained within the range of a vacuum degree of 6±1 KPa and a temperature of 240±1°C. After the pre-condensation reaction is carried out for 2.5 hours, the reaction is stopped, and the excess diol in the pre-condensation kettle is discharged to obtain a pre-condensation product.
[0073] The final polycondensation reaction is carried out as follows: the pre-polycondensation product is introduced into the final polycondensation kettle, the final polycondensation kettle is evacuated, and the final polycondensation kettle is heated. The reaction environment in the final polycondensation kettle is maintained within the range of a vacuum degree of 150±1Pa and a temperature of 283±1°C, and the polycondensation reaction is carried out for 2.5 hours, and then the reaction is stopped to obtain a final polycondensation product.
[0074] The molding operation is as follows: the final polycondensation product is pumped into the die head, and then the final polycondensation product is cast through the die head onto a cooling roller at 13°C to obtain a cast sheet. At the same time, a leeward device is used to blow air on the side of the cast sheet away from the cooling roller. The blowing temperature is 4°C and the wind speed is 4m / s. After cooling and molding, the cast sheet is sent to a longitudinal stretching machine, the cast sheet is first preheated at 65°C, and then the temperature of the cast sheet is heated to 80°C by infrared heating, and then 3.3 times longitudinal stretching is performed. After the longitudinal stretching is completed, it is cooled and shaped at 13°C to obtain a longitudinal drawn sheet, and then the longitudinal drawn sheet is placed in an oven, preheated at 70°C, and then placed in a transverse stretching machine, and 3.4 times transverse stretching is performed at 25°C. After the transverse stretching is completed, a transverse sheet is obtained, the transverse sheet is subjected to high-temperature shaping treatment at 175°C, and then cooled and trimmed at 25°C, and finally rolled up after corona treatment to obtain a white solar backplane base film.
[0075] Comparative Example 2 This comparative example provides a method for forming a solar backplane base film, using the following steps: The slurry is prepared by the following operation: terephthalic acid and ethylene glycol are added into a pulping kettle at a weight ratio of 1:1.42, and stirred and pulped until uniform to obtain a slurry.
[0076] The catalyst liquid is prepared by the following operation: ethylene glycol and antimony trioxide are added into a preparation kettle at a weight ratio of 50:1, stirred until uniform, and the temperature in the preparation kettle is heated to 182° C. to react to obtain the catalyst liquid.
[0077] The esterification product is prepared as follows: the slurry and the catalyst liquid are added into the esterification kettle at a weight ratio of 92.3:7.2, and stirred until uniform. The temperature in the esterification kettle is heated to 260° C. and the reaction is carried out at a constant temperature for 4.5 hours. The heating is stopped to obtain the esterification product.
[0078] The pre-condensation reaction is carried out as follows: the esterified product, mica particles with a particle size of 0.1-0.7 μm and PET slices are introduced into a pre-condensation kettle in a mass ratio of 4:0.21:0.79, and mixed until uniform to obtain a mixture, in which the mass fraction of the additive melt in the mixture is 20%, and then the pre-condensation kettle is evacuated and heated, and the reaction environment in the pre-condensation kettle is maintained within the range of a vacuum degree of 6±1 KPa and a temperature of 240±1°C. After the pre-condensation reaction is carried out for 2.5 hours, the reaction is stopped, and the excess diol in the pre-condensation kettle is discharged to obtain a pre-condensation product.
[0079] The final polycondensation reaction is carried out as follows: the pre-polycondensation product is introduced into the final polycondensation kettle, the final polycondensation kettle is evacuated, and the final polycondensation kettle is heated. The reaction environment in the final polycondensation kettle is maintained within the range of a vacuum degree of 150±1Pa and a temperature of 283±1°C, and the polycondensation reaction is carried out for 2.5 hours, and then the reaction is stopped to obtain a final polycondensation product.
[0080] The molding operation is as follows: the final polycondensation product is pumped into the die, and then the final polycondensation product is cast through the die onto a cooling roller at 35°C to obtain a cast sheet. At the same time, a leeward device is used to blow air on the side of the cast sheet away from the cooling roller. The blowing temperature is 35°C and the wind speed is 22m / s. After cooling and molding, the cast sheet is sent to a longitudinal stretching machine, the cast sheet is first preheated at 95°C, and then the temperature of the cast sheet is heated to 120°C by infrared heating, and then 3.3 times longitudinal stretching is performed. After the longitudinal stretching is completed, it is cooled and shaped at 35°C to obtain a longitudinal drawn sheet, and then the longitudinal drawn sheet is placed in an oven, preheated at 125°C, and then placed in a transverse stretching machine, and 3.4 times transverse stretching is performed at 145°C. After the transverse stretching is completed, a transverse sheet is obtained, the transverse sheet is subjected to high-temperature shaping treatment at 255°C, and then cooled and trimmed at 185°C, and finally rolled up after corona treatment to obtain a white solar backplane base film.
[0081] Comparative Example 3 This comparative example provides a method for forming a solar backplane base film, which adopts the following steps: The PET slices are added into a screw extruder, melted in a temperature range of 260-280°C, and then extruded to obtain a PET polyester film. A 50 μm thick organic fluorine epoxy resin layer is then coated on the surface of the PET polyester film. After curing, a white solar backplane base film is obtained.
[0082] Performance testing The following performance tests were performed on the base film samples prepared in Examples 1-36 and Comparative Examples 1-3: Quality indicators of the final polycondensation product or the final polycondensation melt: The final polycondensation products of Examples 1-30, Examples 35-36 and Comparative Examples 1-3, and the final polycondensation melts of Examples 31-34 were tested, and it was found that the quality indicators of the final polycondensation products of Examples 1-30, Examples 35-36 and Comparative Examples 1-3, and the final polycondensation melts of Examples 31-34 were all within the following ranges: intrinsic viscosity 0.80dl / g-0.90dl / g, terminal carboxyl group ≤20mmol / kg, melting point 250℃-272℃, ash content 1.0%-5.0%.
[0083] Morphology: The thickness of the base film samples was measured with a digital micrometer and found to be 275 μm. The test environment was 25° C. and 60% humidity. Then, the appearance of the base film samples was observed.
[0084] Tensile strength: According to the provisions of Chapter 11 of GB / T13542.2-2009, the tensile strength of the base film sample is tested, where the strip width is 15 mm, the tensile speed is 100 mm / min, the marking interval is 100 mm, and the clamping distance of 100 mm can also be selected when there is no dispute.
[0085] Elongation at break: According to the provisions of Chapter 23 of GB / T13542.2-2009, the elongation at break of the base film sample is tested. The resolution of the measuring instrument shall not be less than 0.1mm. The test conditions are heating temperature of 150±2℃ and heating time of 30min.
[0086] Thermal shrinkage rate: According to the provisions of Chapter 23 of GB / T13542.2-2009, the resolution of the measuring instrument shall not be less than 0.1mm. Test conditions: heating temperature is (150 ± 2°C, heating time is 30min.
[0087] Light transmittance: Use a light transmittance meter to test the light transmittance of the base film sample at a wavelength of 400-1100nm.
[0088] Water vapor transmission rate: The water vapor transmission rate of the base film sample is tested in a test environment of temperature (38±2)°C and relative humidity (90±2)%.
[0089] High temperature and high pressure test: test conditions: 121℃, 100% humidity, 0.2Mpa, aging for 48h and 72h.
[0090] UV aging test: under ultraviolet light in the range of 280nm to 385nm, the total irradiation amount reaches 180kwh / m 2 Finally, the mechanical properties and yellowing were tested.
[0091] The above test results are shown in Table 1 and Table 2.
[0092] Table 1 Table 2 Combining Example 1 and Comparative Examples 1-3 and Table 1-2, it can be seen that compared with Example 1, the appearance of Comparative Examples 1-2 is warped, the tensile strength and elongation at break of Comparative Examples 1-3 are both small, the heat shrinkage of Comparative Examples 1-3 is large, the light transmittance of Comparative Example 3 is too large, and the water vapor permeability of Comparative Examples 1 and 3 is too large. Moreover, Comparative Examples 1-3 all suffered brittle fracture after aging at high temperature and high pressure for 72 hours, and the elongation at break was small after the light aging test, and the yellowing was large. This shows that under the preparation method and process conditions of Example 1 of the present application, it is helpful to simultaneously improve the mechanical properties, high temperature and high pressure resistance and light aging resistance of the base film, reduce the heat shrinkage and water vapor permeability, and compared with the fluorine-containing base film of Comparative Example 3, the base film of Example 1 of the present application does not contain fluorine, and the performance is still relatively excellent.
[0093] It can be seen from Examples 1-9 and Tables 1-2 that the various indicators of the base films of Examples 1-9 are slightly different, which means that the base films of Examples 1-9 have good mechanical properties, high temperature and high pressure resistance, and light aging resistance. Within the process conditions of Examples 1-9, fluorine-free base films with excellent performance can be prepared.
[0094] From Example 1, Examples 10-13 and Tables 1-2, it can be seen that compared with Example 1, the various indicators of the base film of Examples 10-11 do not change much, the heat shrinkage rate of the base film of Examples 12-13 is significantly increased, and the elongation at break of the base film of Examples 12-13 is significantly reduced and the yellowing is increased after the high temperature and high pressure resistance test and the light aging resistance test. This shows that within the process conditions of Examples 1 and 10-11, the performance of the base film can be further improved.
[0095] Combining Example 1, Examples 14-17 and Tables 1-2, it can be seen that compared with Example 1, the various indicators of the base membranes of Examples 14-17 do not change much, which shows that the use of the above-mentioned weight ratio of slurry and catalyst liquid and esterification temperature are helpful to prepare a fluorine-free base membrane with excellent performance.
[0096] It can be seen from Example 1, Examples 18-22 and Tables 1-2 that compared with Example 1, the various indicators of Examples 18-19 and Example 22 have not changed much. After the high temperature and high pressure resistance test and the light aging resistance test, the mechanical properties and yellowing of the base film of Examples 20-21 are worse. This shows that the raw material ratios and raw material types of Example 1, Examples 18-19 and Example 22 can help further improve the high temperature and high pressure resistance and light aging resistance of the base film.
[0097] Combining Example 1, Example 23-36 and Table 1-2, it can be seen that compared with Example 1, the tensile strength and elongation at break of Examples 23-24, Examples 27-28, and Examples 31-36 are higher, the heat shrinkage is lower, and the mechanical properties and yellowing are better after the high temperature and high pressure test and the light aging test, while the mechanical properties and yellowing of the base film of Examples 25-26 and Examples 29-30 are poor after the high temperature and high pressure test and the light aging test. This shows that controlling the process conditions within the range of Example 1, Examples 23-24, Examples 27-28, and Examples 31-36 is helpful to improve the high temperature and high pressure resistance and light aging resistance of the base film.
[0098] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A method for manufacturing a white solar backplane base film by a direct melting method, characterized in that: The following steps are involved: Slurry preparation: mixing one of the dicarboxylic acid or the dimethyl dicarboxylate with the diol to obtain a slurry; Preparation of catalyst liquid: dissolving the catalyst in diol to obtain catalyst liquid; Preparation of esterification product: Mix the slurry and the catalyst solution, heat to 160-265°C and react for 4-5 hours to obtain the esterification product; Preparation of additive melt: melt-blending the inorganic particle additive and the polyester chips at 260-280° C. to obtain the additive melt; Pre-condensation: The esterification product and the additive melt are mixed, and a pre-condensation reaction is carried out in a vacuum environment at 200-280°C, and then the excess diol is discharged to obtain a pre-condensation product; Final polycondensation: subjecting the pre-polycondensation product to a polycondensation reaction in a vacuum environment at 280-285°C to obtain a final polycondensation product; Molding: The final polycondensation product is pumped into the die head, and after sheet casting, cooling molding, longitudinal stretching, transverse stretching, heat setting and corona treatment, a white solar backplane base film is obtained.
2. The method for manufacturing a white solar backplane base film by direct melting method according to claim 1, characterized in that: In the slurry making step, when a dicarboxylic acid is mixed with a diol, the molar ratio of the dicarboxylic acid to the diol is 1:1.15-1:1.7, and when a dimethyl dicarboxylate is mixed with a diol, the molar ratio of the dimethyl dicarboxylate to the diol is 1:1.8-1:2.4; the dicarboxylic acid includes at least one of terephthalic acid and isophthalic acid, the dimethyl dicarboxylate includes at least one of ethylene terephthalate, ethylene isophthalate and ethylene naphthalate, and the diol includes at least one of ethylene glycol, neopentyl glycol, propylene glycol, butanediol and 1,4-cyclohexanedimethanol.
3. The method for manufacturing a white solar backplane base film by direct melting method according to claim 2, characterized in that: In the step of preparing the catalyst liquid, the diol is ethylene glycol, and the diol and the catalyst are mixed in a weight ratio of 100:(1-3), and dissolved at 175-188° C. to obtain a catalyst liquid; when a dicarboxylic acid is mixed with the diol, the catalyst is antimony trioxide; when a dimethyl dicarboxylate is mixed with the diol, the catalyst is a mixture of one or more of calcium acetate, cadmium acetate, zinc acetate, magnesium acetate, and cobalt acetate.
4. The method for manufacturing a white solar backplane base film by direct melting method according to claim 3, characterized in that: In the esterification product preparation step, the slurry and the catalyst liquid are mixed in a weight ratio of (87.5-98):(2-12.5).
5. The method for manufacturing a white solar backplane base film by direct melting method according to claim 1, characterized in that: In the step of preparing the additive melt, the particle size of the inorganic particle additive is 0.1-0.7 μm, the weight ratio of the inorganic particle additive to the polyester chip is (4-50):100, and the inorganic particle additive includes at least one of mica, barium sulfate, kaolin, titanium dioxide, calcium carbonate, silicon dioxide, talc and montmorillonite.
6. The method for manufacturing a white solar backplane base film by direct melting method according to claim 5, characterized in that: In the pre-polycondensation step, the esterified product and the additive melt are mixed to obtain a mixture, the mass fraction of the additive melt in the mixture is 10%-30%, and the pre-polycondensation reaction is carried out at a vacuum degree of 1-10KPa and a temperature of 270-280°C for 2-3h, and then the excess diol is discharged to obtain a pre-polycondensation product.
7. The method for manufacturing a white solar backplane base film by direct melting method according to claim 1, characterized in that: In the final polycondensation step, the pre-polycondensation product is subjected to a polycondensation reaction at a vacuum degree of 100-200 Pa and a temperature of 280-285° C. for 2-3 hours to obtain a final polycondensation product.
8. The method for manufacturing a white solar backplane base film by direct melting method according to claim 7, characterized in that: The final polycondensation step also includes the following steps: mixing the final polycondensation product with an online viscosity enhancer until uniform to obtain a final polycondensation melt, the quality indicators of the final polycondensation melt are as follows: intrinsic viscosity 0.80dl / g-0.90dl / g, terminal carboxyl group ≤20mmol / t, melting point 250℃-272℃, ash content ≤0.06%; in the molding step, pumping the final polycondensation melt into the die head.
9. The method for manufacturing a white solar backplane base film by direct melting method according to claim 8, characterized in that: The mass fraction of the online viscosity enhancer in the final polycondensation melt is 0.2%-3.0%, and the online viscosity enhancer includes any one of oxazoline, isocyanate, pyromellitic anhydride, trimellitic anhydride, and glycidyl ether epoxy compounds.
10. A white solar back sheet base film, characterized in that: The white solar back panel base film is prepared by the direct melting method as described in any one of claims 1 to 9.
Citation Information
Patent Citations
Polyester film, and solar-cell back sheet and solar cell each including same
CN102470653A
Preparation method of polyester chip for solar battery back film
CN105542138A
Solar battery backplane, and preparation method of film polyester used for backplane
CN106008940A
Preparation method of PET resin for solar cell backboard film directly produced by liquid phase polymerization
CN113698745A
White film for Solar Cell Module and Manufacturing method thereof
KR1020120119301A