Preparation method of PMMA radiation refrigeration film doped with TiO2 particles
By using the scraping method, the PMMA radiation refrigeration film doped with TiO2 particles is prepared, which improves the reflection and emissivity of the material, solves the problems of power consumption of traditional refrigeration equipment and the increase in the temperature of radiated materials, and achieves a significant cooling effect. Broad prospects for refrigeration in buildings.
Patent Information
- Application Number
- CN202410984318.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-12-06
AI Technical Summary
The widespread use of traditional refrigeration equipment has led to a surge in power demand, and radiated refrigeration materials are prone to absorb the irradiance of the influx of the daytime sunlight, resulting in an increase in temperature, making it difficult to achieve effective daytime radiation refrigeration.
The PMMA radiation refrigeration film doped with TiO2 particles is prepared by scraping coating method, and the ratio of PMMA, acetone and deionized water is used to improve the reflectivity and emissivity of the material, and the effective reflection and emission of heat are achieved.
The PMMA radiation refrigeration film doped with TiO2 particles shows high reflectivity and emissivity in the visible and mid-infrared light bands, effectively reducing the temperature, with a significant average cooling effect, with a maximum temperature difference of 22.1℃, and shows good results in practical applications. Radiation refrigeration performance.
Smart Images

Figure CN119081173A_ABST
Abstract
Description
Technical Field
[0001] A doped TiO 2 The invention discloses a method for preparing a PMMA radiation cooling film of particles, which belongs to the fields of materials and energy, and mainly involves the cooling problem of ambient temperature. The radiation cooling film can effectively reduce the ability of sub-ambient temperature. Background Art
[0002] In order to get a little comfort in the hot season, people generally tend to use cooling equipment such as air conditioners. The large-scale use of cooling equipment such as air conditioners has led to a surge in electricity demand, and traditional electricity production methods usually rely on fossil fuels, which further exacerbates the trend of global warming and causes irreversible damage to the earth's climate system.
[0003] Radiative cooling is a cooling technology that can spontaneously dissipate heat and cool down without consuming electricity or other energy. It radiates heat from the earth to outer space with a temperature of about 3K through the atmospheric transparent window (8-13μm). Therefore, people pursue materials with excellent radiation to achieve cooling, but under direct sunlight during the day, most thermal radiation materials exposed to the outside will absorb the incident irradiance, causing the temperature to rise. Therefore, to achieve daytime radiative cooling, it is also necessary to have good sunlight reflection performance to reflect the heat as much as possible, so that the radiated heat is greater than the absorbed heat, and cooling is achieved. Summary of the invention
[0004] A doped TiO 2 Preparation method of PMMA radiation cooling film with particles, wherein the radiation cooling film is composed of PMMA, acetone, deionized water and TiO 2 The sample was prepared by scraping method, and the sample showed a reflectivity of 91% (0.4-1.5μm) and an emissivity of 98% (2.5-25μm), among which TiO 2 Sample temperature of particles not doped with TiO 2 The particle temperature dropped by an average of 7.6°C, with a maximum temperature difference of 9.2°C, and dropped by an average of 17.4°C from the ambient temperature, with a maximum temperature difference of 22.1°C. Because the invented material is inexpensive and the preparation method is simple, the film has broad application prospects in building cooling.
[0005] A PMMA-doped TiO 2 Preparation method of particle radiation refrigeration film.
[0006] The preparation method of this type of coating includes the following substances: PMMA solid particles (Shanghai McLean), acetone (Chengdu Cologne Chemical), TiO 2 (Anhui Bangrui New Materials), deionized water.
[0007] PMMA (Shanghai McLean) was used as the substrate, acetone (Chengdu Cologne Chemical) was used as the solvent, and deionized water was used as the non-solvent. TiO 2 The particle and radiation cooling film are prepared by a non-solvent induced phase separation method, and the specific preparation steps are as follows: (1) Preparation of PMMA solution: Add PMMA crystals to acetone and mix at 40-65°C for 0.5-1h, preferably at 50°C, to obtain a translucent solution.
[0008] (2) Preparation of mixed PMMA solution: Add deionized water and TiO 2 , keep the temperature constant, and stir magnetically for 2-3 hours to make it disperse evenly to obtain a white solution; (3) Cleaning of acrylic sheets: First, clean the acrylic sheets with laundry water, then ultrasonicate them in clean water, then clean them with anhydrous ethanol, then clean them with deionized water, and finally dry them for later use.
[0009] (4) Coating film formation: drip the white solution in step (2) onto the surface of the cleaned and dried acrylic sheet in step (3), then use a scraper to evenly scrape the solution to form a smooth coating. Finally, place the sample in a room temperature environment to dry to obtain doped TiO 2 PMMA radiative cooling film with particles.
[0010] The prepared doped TiO 2 PMMA radiative cooling film with TiO 2 The particles account for 1-10% of the volume of the PMMA radiative cooling film.
[0011] The PMMA: acetone: deionized water: TiO 2 The added mass ratio is 0.3~1: 2.4~20: 0.3~1:0.2~1.
[0012] TiO in step (1) 2 The particle size is 0.5-2μm.
[0013] The thickness of the radiative cooling film in step (4) is set to 500 μm plus the thickness of the 1000 μm acrylic plate so the final thickness is 1500 μm.
[0014] Advantages of patents: The PMMA radiation cooling film prepared by doping titanium dioxide particles effectively improves the radiation capacity of PMMA in the atmospheric transparent window in the mid-infrared light band (8-13um), making the radiation cooling film have a high reflectivity in the entire solar band: the visible light band (0.4-1.5um), and a high emissivity in the mid- and far-infrared light bands (3-25um). This makes the radiation cooling film have a good radiation cooling effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 Example 1: Reflectivity diagram of titanium dioxide doped with different mass fractions.
[0016] Figure 2 Example 1: Emissivity graph comparing two ratios.
[0017] Figure 3 Actual picture of the test device of Example 2.
[0018] Figure 4 Example 2 Schematic diagram of the structure of the testing device.
[0019] Figure 5 Example 2: Daytime test temperature diagram of the radiative cooling film without and with titanium dioxide particles.
[0020] Figure 6 Example 2 Test the wind humidity on the day.
[0021] Figure 7 Example 3: Actual picture of the radiation cooling film used in the outdoor unit of the air conditioner.
[0022] Figure 8 Example 3: Temperature comparison chart of the radiant cooling film and the air conditioner outdoor unit captured by thermal infrared imaging. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in conjunction with the embodiments of the present invention.
[0024] Example 1 Effect of doping titanium dioxide particles with different mass fractions on radiative cooling films (1) PMMA was chosen as the substrate for radiative cooling because it has a very good radiation emissivity. This property is crucial for radiative cooling because radiative cooling relies on the ability to effectively emit heat into outer space in the form of infrared radiation. Another important concern is cost-effectiveness. PMMA is more economical than other high-performance materials, which makes it possible to achieve efficient radiative cooling while controlling costs.
[0025] (2) TiO2 particles themselves have a very high refractive index, which means that they can strongly reflect sunlight and reduce heat absorption. At the same time, TiO2 particles have a good ability to absorb ultraviolet rays in the ultraviolet band, which can reduce the heat caused by ultraviolet rays, effectively block ultraviolet rays, and enhance the weather resistance of the material.
[0026] (3) The present invention studies the effect of changing the mass fraction of titanium dioxide particles on the optical properties of the film (i.e., the mass fraction of titanium dioxide particles added during preparation in the PMMA radiation cooling film). By setting the thickness of the radiation cooling film to 500 μm and the particle size to 1 μm, the present invention conducts experiments on the preparation of films with five mass fractions of 1%, 3%, 5%, 7% and 9%. The reflectivity optical properties of several film materials are studied, and the results of the five ratios of sunlight reflectivity are shown in the attached figure. Figure 1 shown. (4) For the five samples prepared above, characterize the optical properties and compare the reflectivity curves, as shown in the attached figure. Figure 1 As shown. By comparing the curve groups, we can see that the overall trend of the doping ratio from 1% to 9% is to rise first and then fall. In the visible light band (0.4-0.78μm), the 9% ratio is slightly higher than 5%, but the reflectivity is lower than 5% in the near-infrared band (0.78-2.5μm). The reflectivity of the ratios of 5% and 7% in the visible light and near-infrared bands is not much different. Figure 2 From the 5% and 7% emissivity, it can be seen that 5% is significantly higher than 7% in the 8-13μm band of the atmospheric window. Considering all factors, 5% is the best ratio.
[0027] (5) This shows that by changing the ratio of PMMA film material embedded with TiO2 particles, the reflectivity of PMMA radiative cooling film will be improved. By improving the reflectivity of PMMA radiative cooling film, the cooling effect of this film is further achieved. In the 0.4-1.5μm band, including the visible light band, the average reflectivity is greater than 0.91. Considering the ratios of the five doped titanium dioxide particles, we finally chose 5% doped titanium dioxide as the optimal ratio.
[0028] Example 2 PMMA doped with TiO 2 Particles are not doped with TiO 2 PMMA radiation cooling temperature comparison of particles (1) Preparation of PMMA solution: Mix 0.5 g of PMMA crystal particles and 4.0 g of acetone, heat to 45 °C, and stir magnetically for 1 h to form a translucent solution.
[0029] (2) Preparation of mixed solution: Add 0.3 g of titanium dioxide with a particle size of 1 μm to the above solution and continue magnetic stirring for 1.5 h to make it evenly dispersed to obtain a white solution.
[0030] (3) Cleaning of acrylic sheets: First, clean the acrylic sheets with laundry water, then ultrasonicate them in clean water, then clean them with anhydrous ethanol, then clean them with deionized water, and finally dry them for later use.
[0031] (4) Coating film formation: The white solution in step (2) is dropped onto the surface of the cleaned and dried acrylic sheet in step (3), and then the solution is evenly scraped with a scraper to form a smooth coating. Finally, the sample is placed in a room temperature environment to dry to obtain doped TiO 2 PMMA radiative cooling film with particles.
[0032] (5) Three identical devices were built as shown in the attached Figure 3 As shown, it is used to compare the conditions without sample, with sample and without TiO 2 The refrigeration performance of the particle sample. The structural diagram of the test device is shown in the attached figure. Figure 4 As shown, the overall size of the test box is 15cm×15cm×15cm, and there is a hole in the center of the top, which is 5cm×5cm×5cm, as an isolation space for sample testing. The outside of the test box is wrapped with aluminum foil, and the inside is filled with polystyrene foam, which mainly serves to isolate the convection and conduction heat dissipation from the outside.
[0033] (6) The experiment was conducted in Yichang in October under clear weather. The test box was placed horizontally as shown in the attached figure. Figure 3 As shown, no sample film is placed and undoped TiO 2 Particles and placement of doped TiO 2 The PMMA radiation cooling film with particles was compared with the test case. The temperature results tested in the test box are shown in the attached Figure 5 As shown, the daytime test recorded the temperature change from 10:40 to 15:00, with Figure 3 The thermocouple in the test chamber detected the sub-ambient temperature (i.e., the cavity temperature where the sample film is not placed). 2 Particle temperature and undoped TiO 2 Particle temperature. Figure 5 Medium temperature test data, doped TiO 2 The particle temperature was lower by an average of 17.4°C than the subambient temperature of the blank sample, reaching a maximum temperature difference of 22.1°C at 12:13 noon, which was lower than that of the undoped TiO 2 The temperature of the particles dropped by an average of 7.6°C, reaching a maximum temperature difference of 9.2°C at 12:35 noon. The wind and humidity on the day of the test were as follows: Figure 6 As shown, the average humidity is 32% and the wind speed is 1m / s.
[0034] (7) Through the above radiation cooling film and undoped TiO 2The temperature test of the particles showed that: in the daytime test, the TiO 2 The sample temperature of the particles was lower than the ambient temperature by an average of 17.4°C, with a maximum temperature difference of 22.1°C, which was lower than that of the undoped TiO 2 The particle temperature decreased by an average of 7.6°C, with a maximum temperature difference of 9.2°C. 2 Particle radiation cooling film is better than undoped TiO 2 The particles have a relatively obvious radiation cooling effect.
[0035] Example 3 Doped TiO 2 Application of PMMA radiation cooling film in outdoor power equipment (1) Preparation of PMMA solution: Mix 0.5 g of PMMA crystal particles and 4.0 g of acetone, heat to 45 °C, and stir magnetically for 1 h to form a translucent solution.
[0036] (2) Preparation of mixed solution: Add 0.3 g of titanium dioxide with a particle size of 1 μm to the above solution and continue magnetic stirring for 1.5 h to make it evenly dispersed to obtain a white solution.
[0037] (3) Cleaning of acrylic sheets: First, clean the acrylic sheets with laundry water, then ultrasonicate them in clean water, then clean them with anhydrous ethanol, then clean them with deionized water, and finally dry them for later use.
[0038] (4) Coating film formation: The white solution in step (2) is dropped onto the surface of the cleaned and dried acrylic sheet in step (3), and then the solution is evenly scraped with a scraper to form a smooth coating. Finally, the sample is placed in a room temperature environment to dry to obtain doped TiO 2 PMMA radiative cooling film with particles.
[0039] (5) Prepared doped TiO 2 The PMMA radiation cooling film with particles is pasted on the surface of the air conditioner outdoor unit using double-sided tape. Figure 7 As shown, place it outdoors and expose it to the air, and take thermal infrared images to compare the temperature, as shown in the attached Figure 8 As shown, according to the temperature data taken by thermal infrared imaging, doped TiO 2 The surface temperature of PMMA radiation cooling film with particles is 5℃ lower than that of the air conditioner outside unit, which can be explained by the doping of TiO 2 The PMMA radiation cooling film with particles still has good radiation cooling performance and application performance in practical applications.
Claims
1. A method for preparing a PMMA radiation cooling film doped with TiO2 particles, characterized in that: The method comprises the following preparation steps: (1) Preparation of PMMA solution: Add PMMA crystals into acetone to obtain a translucent solution; (2) Preparation of mixed PMMA solution: Add water and TiO2 to the solution prepared in step (1), keep the temperature constant, and disperse it evenly to obtain a white solution; (3) Cleaning of acrylic sheet: First, clean the acrylic sheet with laundry water, then ultrasonicate it in clean water, then clean it with anhydrous ethanol, then clean it with deionized water, and finally dry it for later use; (4) Coating film formation: drip the white solution in step (2) onto the surface of the washed and dried acrylic sheet in step (3), then use a scraper to evenly scrape the solution to form a smooth coating. Finally, place the sample in a room temperature environment to dry to obtain a PMMA radiative cooling film doped with TiO2 particles.
2. The method for preparing the PMMA radiation cooling film doped with TiO2 particles according to claim 1, characterized in that: In step (1), the mixture is mixed at 40-65° C. for 0.5-1 h.
3. The method for preparing the PMMA radiation cooling film doped with TiO2 particles according to claim 1, characterized in that: The particle size of TiO2 in step (2) is 0.5-2 μm.
4. The method for preparing the PMMA radiation cooling film doped with TiO2 particles according to claim 1, characterized in that: PMMA radiation cooling film doped with TiO2 particles, wherein the TiO2 particles account for 1-10% of the mass fraction of the PMMA radiation cooling film.