High-strength biodegradable composite film and preparation method thereof
By hydrophobic modification of cellulose nanocrystals, their compatibility with PBAT, PLA and PCL is improved, and the problems of uneven dispersion and insufficient mechanical properties of cellulose nanocrystals in composite materials are solved, thereby achieving high fracture The production of biodegradable composite films with strength has expanded its application range.
Patent Information
- Application Number
- CN202411481218.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-23
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The insufficient compatibility between cellulose nanocrystals and hydrophobic polymers such as PBAT, PLA and PCL leads to uneven dispersion and insufficient mechanical properties in composite materials, limiting the application of biodegradable polymer films.
Through hydrophobic modification technology, surface modification of cellulose nanocrystals is introduced, surface modification agents such as tannin acid, gallic acid, and caffeic acid, and hydrophobic modifiers such as n-octylamine, decylamine, and dodecylamine are introduced to change their surface properties and improve their Compatibility with PBAT, PLA, PCL, and high-break strength biodegradable composite films are prepared through solutions casting and other processes.
It significantly improves the uniform dispersion and mechanical properties of cellulose nanocrystals in polymer matrix, improves the fracture strength and comprehensive performance of biodegradable polymer films, overcomes compatibility and dispersion problems, and expands its further Multi-field application.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a method for preparing a high-strength biodegradable composite film. Background Art
[0002] Polybutylene adipate terephthalate (PBAT), polylactic acid (PLA) and polycaprolactone (PCL) are three biodegradable polymers that have attracted much attention. Each of them has unique properties and broad application prospects, but also has some inherent limitations.
[0003] Polybutylene adipate terephthalate (PBAT) occupies an important position in the field of environmentally friendly materials due to its good ductility, heat resistance, impact resistance and excellent biodegradability. However, the slow crystallization rate, relatively low fracture strength and poor dimensional stability of PBAT materials have seriously restricted its large-scale application in key areas such as food packaging and agricultural mulch. Although blending modification is regarded as an effective strategy to improve the performance of PBAT, simple direct blending is often difficult to completely overcome its inherent defects. Polylactic acid (PLA), a biodegradable plastic derived from renewable resources, has excellent biocompatibility and degradability, as well as good mechanical properties and processing properties. However, PLA is brittle, lacks toughness, and is easily decomposed at high temperatures, which limits its application in some fields. In addition, PLA has a slow crystallization rate and low crystallinity, which easily leads to unstable product size, further affecting its performance and application range. Polycaprolactone (PCL) is known for its good flexibility and biocompatibility. PCL also has a slow degradation rate, which is suitable for biomedical applications that need to exist for a long time. However, PCL has poor heat resistance and is easy to soften at high temperatures, which limits its use in applications that need to withstand higher temperatures. In addition, the mechanical properties of PCL are relatively weak, especially in terms of tensile strength and hardness, which affects its potential as a structural material.
[0004] Cellulose nanocrystals (CNC), as a new type of green nanomaterial derived from renewable biomass resources, have unique advantages such as high aspect ratio, large specific surface area, high crystallinity and excellent mechanical properties. They are ideal nano-reinforcement materials for improving the performance of the above-mentioned biodegradable polymers. However, the abundant hydroxyl groups on the surface of CNC make it highly hydrophilic, easy to form intramolecular and intermolecular hydrogen bonds, which in turn induce agglomeration and limit its uniform dispersion in composite materials. In addition, CNC has poor compatibility with hydrophobic polymer matrices such as PBAT, PLA and PCL, and it is difficult to fully exert its reinforcement effect as a nano-reinforcement material. Therefore, how to effectively improve the dispersibility and compatibility of CNC in hydrophobic polymers has become a key challenge to improve the mechanical properties of the corresponding polymer films.
[0005] In view of the problems existing in the above technical background, the present invention proposes an innovative solution: optimizing the surface properties of CNC through hydrophobic modification technology, reducing its hydrophilicity, enhancing its compatibility with polymer matrices such as PBAT, PLA and PCL, and thus achieving uniform dispersion of CNC in the polymer matrix. On this basis, the modified CNC is blended with PBAT, PLA or PCL to prepare a biodegradable composite film with high breaking strength and good comprehensive performance. This solution not only overcomes the problem of uneven dispersion and poor compatibility of CNC in composite materials, but also significantly improves the mechanical properties, heat resistance and dimensional stability of biodegradable polymers, providing strong support for the application of biodegradable materials in a wider range of fields. Summary of the invention
[0006] The present invention aims to solve the problem of insufficient compatibility between CNC (cellulose nanocrystals) and various biodegradable polymer matrices (including PBAT (polybutylene adipate terephthalate), PLA (polylactic acid) and PCL (polycaprolactone)). This lack of compatibility makes it difficult to effectively improve the mechanical properties of the film. To this end, the present invention proposes an innovative method for preparing a biodegradable composite film by hydrophobic modification of CNC, which aims to prepare a film with high fracture strength and excellent comprehensive performance. In order to achieve the above objectives, the present invention adopts the following technical solutions: The core of the present invention is to prepare a high-strength biodegradable composite film, and the specific steps include: first, hydrophobically modifying cellulose nanocrystals by introducing three surface modifiers, tannic acid, gallic acid, and caffeic acid, and three hydrophobic modifiers, n-octylamine, decylamine, and dodecylamine, to change their surface properties; then, blending the modified cellulose nanocrystals with PBAT, PLA, and PCL solutions, and preparing them into films by solution casting or other suitable molding processes.
[0007] The specific implementation steps of the above technical solution are as follows: 1. Hydrophobic modification of cellulose nanocrystals: The aqueous dispersion of CNC is concentrated to 1 wt%-3 wt%, and ultrasonic treatment is performed to ensure uniform dispersion; a buffer solution is then added to the concentrated CNC suspension to adjust the pH value to 7.5-9; the CNC suspension with adjusted pH value is poured into a reaction container, and a certain amount of surface modifier (one or more of tannic acid, gallic acid or caffeic acid, the amount of which is 3 wt%-7 wt% based on the mass of CNC) is added. After sufficient stirring for 6-8 hours, a hydrophobic modifier (one or more of n-octylamine, decylamine or dodecylamine, the amount of which is 100 wt%-300 wt% based on the mass of CNC) is added, and stirring is continued for 2-5 hours; unreacted residues are removed by centrifugation, and the product is then washed multiple times with deionized water and ethanol, respectively, to obtain hydrophobically modified cellulose nanocrystals (such as CNC-TA-DA, CNC-GA-LA, CNC-CA-OA, etc.).
[0008] 2. Preparation of biodegradable composite films: The hydrophobically modified CNC obtained in step 1 is added to a suitable solvent (N,N-dimethylformamide, chloroform, dichloromethane, etc.) of PBAT, PLA or PCL to ensure that the content of the hydrophobically modified CNC in the solution is 1 wt%-3 wt%; the mixture is stirred at a temperature of 20 ℃-80 ℃ until the hydrophobically modified CNC is uniformly dispersed in the polymer solution; then the uniformly dispersed mixture is poured into a preheated mold and dried to constant weight, thereby obtaining a biodegradable composite film (such as PBAT / CNC-TA-DA, PLA / CNC-GA-LA, PCL / CNC-CA-OA, etc.).
[0009] Compared with the prior art, the present invention has the following significant features: The present invention uses biomass material CNC as filler, which not only enhances the mechanical properties of biodegradable polymer matrix materials such as PLA and PCL, but also embodies the concept of green environmental protection. CNC is derived from natural cellulose materials widely found in nature, and its application helps reduce dependence on traditional petroleum-based plastics.
[0010] Through innovative hydrophobic modification technology, the compatibility and dispersibility between CNC and various biodegradable polymer matrices are significantly improved, thereby effectively improving the mechanical properties of the composite film, especially the breaking strength.
[0011] The preparation method of the present invention is simple, efficient, and easy to industrialize. Moreover, by adjusting the type and amount of the surface modifier and the hydrophobic modifier, the hydrophobic modification effect of CNC can be precisely regulated to meet different application requirements.
[0012] The present invention provides a new solution for the field of biodegradable materials, which is expected to promote the application and development of bio-based materials, and promote environmental protection and sustainable development. In summary, the present invention successfully prepared a biodegradable composite film with high breaking strength by optimizing the hydrophobic modification process of CNC and its blending process with various biodegradable polymers, opening up a new way for the application and development of bio-based materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 is the CNC modification flow chart of Example 1, showing the transformation process from cellulose nanocrystals to hydrophobically modified cellulose nanocrystals.
[0014] Figure 2 This is a physical picture of the biodegradable composite film (PBAT / CNC-TA-DA) prepared in Example 1, showing the transparency and uniformity of the film.
[0015] Figure 3 This is a data comparison chart of the fracture strength and elongation at break of the CNC composite film before and after modification in Example 1. By comparing the performance of the pure PBAT film, the composite film with unmodified CNC and the composite film with CNC-TA-DA, it is shown that the addition of CNC-TA-DA can significantly improve the strength of the PBAT film.
[0016] Figure 4 This is a data comparison chart of the breaking strength and breaking elongation of the CNC composite film before and after modification in Example 2. By comparing the performance of pure PLA film, unmodified CNC composite film and composite film with added CNC-GA-TA-LA, it is shown that the addition of CNC-GA-TA-LA can significantly improve the strength of PLA film. DETAILED DESCRIPTION
[0017] The specific implementation of the technical solution of the present invention is described in detail below, but the present invention is not limited to the following description. The present invention aims to provide a method for preparing hydrophobically modified cellulose nanocrystals and biodegradable composite films thereof, and various performances can be optimized by adjusting reaction conditions and material ratios. Example 1
[0018] (1) Hydrophobic modification of cellulose nanocrystals: In this embodiment, the aqueous dispersion of cellulose nanocrystals is concentrated to 2 wt %, and then ultrasonically treated to disperse evenly. Then, an appropriate amount of buffer solution is added to adjust the pH to 8. The suspension is poured into a three-necked flask, 0.05 g of tannic acid is added, and stirred for 6 hours to allow the tannic acid to bind to the surface of the cellulose nanocrystals. Then 1.88 g of decylamine is added to introduce a hydrophobic group, and the reaction is continued to stir for 3 hours to allow the decylamine to react with the tannic acid on the surface of the cellulose nanocrystals to form a hydrophobic layer. Finally, the unreacted residue is removed by centrifugation, and the obtained product is washed 3 times with deionized water and ethanol respectively to remove impurities to obtain hydrophobic cellulose nanocrystals (CNC-TA-DA).
[0019] (2) Preparation of biodegradable composite films: The hydrophobic cellulose nanocrystals obtained in step (1) were added to the N,N-dimethylformamide solution of PBAT at a ratio of 1 wt%. The mixture was stirred at 60 °C to uniformly disperse the hydrophobic cellulose nanocrystals in the PBAT solution. After uniform dispersion, the mixed solution was poured into a preheated mold and dried to constant weight to obtain a biodegradable composite film (PBAT / CNC-TA-DA). Example 2
[0020] (1) Hydrophobic modification of cellulose nanocrystals: In this embodiment, the aqueous dispersion of cellulose nanocrystals is concentrated to 3 wt%. A buffer solution is added to adjust the pH to 7.5. 0.05 g of gallic acid and 0.02 g of tannic acid are added to a three-necked flask and stirred for 8 hours to allow gallic acid and tannic acid to bind to the surface of the cellulose nanocrystals. Then 2.5 g of dodecylamine is added to introduce hydrophobic groups, and stirring is continued for 4 hours to allow dodecylamine to react with gallic acid and tannic acid on the surface of the cellulose nanocrystals to form a hydrophobic layer. Finally, the unreacted residue is removed by centrifugation, and the obtained product is washed 4 times with deionized water and ethanol respectively to remove impurities to obtain modified hydrophobic cellulose nanocrystals (CNC-GA-TA-LA).
[0021] (2) Preparation of biodegradable composite films: The hydrophobic cellulose nanocrystals obtained in step (1) were added to a chloroform solution of PLA (polylactic acid) at a ratio of 2 wt%. The mixture was stirred at 50 °C to uniformly disperse the hydrophobic cellulose nanocrystals in the PLA solution. After uniform dispersion, the mixed solution was poured into a preheated mold and dried to constant weight to obtain a biodegradable composite film (PLA / CNC-GA-TA-LA). Example 3
[0022] (1) Hydrophobic modification of cellulose nanocrystals: In this embodiment, the aqueous dispersion of cellulose nanocrystals was concentrated to 1.5 wt%. A buffer solution was added to adjust the pH to 8.5. 0.08 g of caffeic acid was added to a three-necked flask and stirred for 5 hours to allow the caffeic acid to bind to the surface of the cellulose nanocrystals. Then 2.0 g of n-octylamine was added to introduce hydrophobic groups, and stirring was continued for 2.5 hours to allow n-octylamine to react with gallic acid on the surface of the cellulose nanocrystals to form a hydrophobic layer. Finally, the unreacted residues were removed by centrifugation, and the obtained product was washed twice with deionized water and ethanol, respectively, to obtain modified hydrophobic cellulose nanocrystals (CNC-CA-OA).
[0023] (2) Preparation of biodegradable composite films: The hydrophobic cellulose nanocrystals obtained in step (1) were added to a dichloromethane solution of PCL (polycaprolactone) and PLA (polylactic acid) at a ratio of 1.5 wt%. Stirring was performed at room temperature to uniformly disperse the hydrophobic cellulose nanocrystals in the PCL-PLA solution. After uniform dispersion, the mixed solution was poured into a preheated mold and dried to constant weight to obtain a biodegradable composite film (PCL-PLA / CNC-CA-OA).
[0024] Note: The above examples are only used to illustrate the technical ideas and technical features of the present invention, and cannot be used to limit the protection scope of the present invention. Any equivalent transformation or modification made according to the essence of the present invention, such as changing the concentration of cellulose nanocrystals, the selection of nanocrystal surface modifiers and hydrophobic groups, the preparation conditions of composite films, etc., should be covered within the protection scope of the present invention.
Claims
1. A method for preparing a high-strength biodegradable composite film, Features The following steps are involved: At least one surface modifier selected from tannic acid, gallic acid, and caffeic acid and at least one hydrophobic modifier selected from n-octylamine, decylamine, and dodecylamine are introduced onto the surface of cellulose nanocrystals (CNC) to perform hydrophobic modification treatment on the CNC; The hydrophobically modified CNC is solution-blended with at least one biodegradable polymer selected from polybutylene adipate terephthalate (PBAT), polylactic acid (PLA) and polycaprolactone (PCL), and is prepared into a high-strength biodegradable composite film by solution casting or other suitable molding processes.
2. A method for preparing a high-strength biodegradable composite film according to claim 1, It is characterized in that The preparation method specifically comprises the following steps: (1) Hydrophobic modification of CNC: The CNC aqueous dispersion is concentrated to a suitable concentration, and after ultrasonic treatment, a buffer solution is added to adjust the pH to a suitable range; subsequently, the suspension is poured into a reaction container, at least one surface modifier is added, and stirred for a certain period of time; at least one hydrophobic modifier is added, and stirring is continued; unreacted products are removed by centrifugation, and the CNC is washed with deionized water and ethanol for multiple times, and then dried to obtain hydrophobically modified CNC; (2) Preparation of composite films: The hydrophobically modified CNC obtained in step (1) is added to a suitable solution of at least one biodegradable polymer selected from PBAT, PLA and PCL, and stirred at a suitable temperature until the hydrophobically modified CNC is uniformly dispersed in the biodegradable polymer solution; the mixture is then poured into a mold preheated to an appropriate temperature and dried to a constant weight to obtain a high-strength biodegradable composite film.
3. The method for preparing a high-strength biodegradable composite film according to claim 2, It is characterized in that In step (1), the concentration of the CNC aqueous dispersion concentrate is 1 wt%-3 wt%; the pH range is 7.5-9; the stirring time after adding the surface modifier is 6-8 hours; the stirring time after adding the hydrophobic modifier is 2-5 hours; the amount of the surface modifier added is 3 wt%-7 wt% based on the mass of CNC; the amount of the hydrophobic modifier added is 100 wt%-300 wt% based on the mass of CNC; and the number of washing times after centrifugation is 2-4 times.
4. The method for preparing a high-strength biodegradable composite film according to claim 2, It is characterized in that In step (2), the content of the hydrophobically modified CNC in the biodegradable polymer solution is 1 wt%-3 wt%; the suitable solvent is N , N -dimethylformamide or chloroform or dichloromethane, the suitable temperature is 20°C-80°C, and the condition for drying to constant weight is to continue drying at the set temperature until the mass no longer changes.
5. A method for preparing a high-strength biodegradable composite film according to any one of claims 1 to 4, It is characterized in that The high-strength biodegradable composite film can be used in the fields of food packaging, agricultural mulch film, biomedical implants, etc.
Citation Information
Patent Citations
Preparation method of hydrophobic nanocellulose material
CN112898441A
Soybean protein-based adhesive, soybean protein-based composite material, and preparation and application of soybean protein-based composite material
CN113512400A
Biodegradable tough composite material and preparation method thereof