Application of superfine fiber / aerogel composite material in sound absorbing material, thermal insulation material or thermal insulation material
Through the preparation method of high-strength hydrogel/microfiber nonwoven composite materials, the problems of insufficient mechanical strength and poor toughness of polyvinyl alcohol aerogel materials are solved, and high-strength, thermal insulation and noise reduction microfiber/gas are achieved. Gel composite material, suitable for sound absorption, insulation and heat insulation materials.
Patent Information
- Application Number
- CN202411187507.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
The existing polyvinyl alcohol aerogel materials have insufficient mechanical strength and poor toughness in actual applications, and it is difficult to achieve uniform fiber dispersion and consistency of aerogel structure in large-scale production, which cannot meet actual needs.
The preparation method of high-strength hydrogel/microfiber nonwoven composite materials includes immersing high-strength hydrogel/microfiber nonwoven composite materials in water and freezing and freezing, through melting, drafting, carding and reinforcement. Prepare microfiber/aerogel composites with high strength and good toughness.
The polyvinyl alcohol aerogel is uniformly filled inside the nonwoven material, forming a structure of mutually covering the aerogel with microfibers as the skeleton. The preparation process is green and environmentally friendly, and has high strength, thermal insulation, noise reduction and ability. Large-scale preparation, suitable for sound absorption, insulation and heat insulation materials.
Smart Images

Figure CN119081215A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of ultrafine fibers and aerogels, and in particular to the application of an ultrafine fiber / aerogel composite material in sound-absorbing materials, heat-preserving materials or heat-insulating materials. Background Art
[0002] Ultrafine fibers and aerogel materials have been widely used in many fields due to their excellent physical and chemical properties. Ultrafine fibers have high specific surface area, good flexibility and strength, and are often used in filtration, thermal insulation and adsorption materials. Aerogels are known for their low density, high porosity and excellent thermal insulation properties, and are widely used in aerospace, building insulation and energy fields.
[0003] Polyvinyl alcohol (PVA) aerogel has become an important aerogel material due to its biocompatibility, renewability and easy processing. However, single PVA aerogel has problems of insufficient mechanical strength and poor toughness in practical applications. Therefore, researchers have tried to compound ultrafine fibers with aerogel to prepare composite materials, thereby improving the performance of aerogel materials. However, on the one hand, the composite material still has problems of insufficient mechanical strength and poor toughness. On the other hand, in large-scale production, it also faces problems such as uniform dispersion of fibers and consistency of aerogel structure, which is difficult to meet the needs of practical applications. In summary, how to prepare a polyvinyl alcohol aerogel composite material with high strength and excellent performance is an urgent problem to be solved. Summary of the invention
[0004] The purpose of the present invention is to overcome the problems existing in the prior art and provide an application of an ultrafine fiber / aerogel composite material in a sound absorbing material, a heat preservation material or a thermal insulation material.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides an application of a superfine fiber / aerogel composite material in a sound absorbing material, a heat preservation material or a heat insulating material. The preparation method of the superfine fiber / aerogel composite material comprises the following steps:
[0007] The high-strength hydrogel / ultrafine fiber nonwoven composite material is immersed in water and frozen, and then freeze-dried to obtain the ultrafine fiber / aerogel composite material.
[0008] Preferably, the method for preparing the high-strength hydrogel / ultrafine fiber nonwoven composite material comprises the following steps:
[0009] (1) melting a first polymer and a second polymer independently to obtain a melt of the first polymer and a melt of the second polymer; and composite spinning the melt of the first polymer and the melt of the second polymer to obtain a water-soluble polyvinyl alcohol bicomponent fiber; wherein the first polymer is thermoplastic polyvinyl alcohol;
[0010] (2) drawing the water-soluble polyvinyl alcohol bicomponent fiber to obtain short fibers;
[0011] (3) combing the short fibers to obtain a polyvinyl alcohol two-component fiber web;
[0012] (4) reinforcing the polyvinyl alcohol two-component fiber web to obtain a water-soluble polyvinyl alcohol two-component carded-needle-punched nonwoven material;
[0013] (5) subjecting the water-soluble polyvinyl alcohol two-component carded-needle-punched nonwoven material to a water-soluble fiber-opening treatment to obtain a solution containing the nonwoven material;
[0014] (6) Mixing the solution containing the nonwoven material and the additive solution, and sequentially performing cross-linking and freezing treatments to obtain the high-strength hydrogel / ultrafine fiber nonwoven composite material.
[0015] Preferably, the weight average molecular weight of the thermoplastic polyvinyl alcohol in step (1) is 5000-8000, the alcoholysis degree of the thermoplastic polyvinyl alcohol is 88-99%, the polymerization degree of the thermoplastic polyvinyl alcohol is 400-1000, and the melt flow index of the thermoplastic polyvinyl alcohol is 25-60 g / 10 min;
[0016] The second polymer includes one or more of polyethylene compounds, polypropylene compounds, polyester compounds, polyamide compounds and polylactic acid compounds;
[0017] The mass fraction of thermoplastic polyvinyl alcohol in the water-soluble polyvinyl alcohol bicomponent fiber is 10-90%.
[0018] Preferably, the freezing environment is a liquid nitrogen environment.
[0019] Preferably, the freeze-drying temperature is -20 to -60°C.
[0020] Preferably, the tensile strength of the ultrafine fiber / aerogel composite material is 10.6-14.0 MPa; the thermal conductivity of the ultrafine fiber / aerogel composite material at 40°C is 0.04061-0.04357 W·m -1 ·K -1 The thermal conductivity at 80°C is 0.04531~0.04762W·m -1 ·K -1The sound absorption coefficient of the ultrafine fiber / aerogel composite material is 0.80-0.84 at 1000HZ, 0.91-0.94 at 2000HZ, and 0.96-0.98 at 4000HZ.
[0021] The beneficial effects of the present invention are:
[0022] In the ultrafine fiber / aerogel composite material prepared by the present invention, polyvinyl alcohol aerogel is uniformly filled inside the non-woven material, realizing the mutual covering between aerogel and ultrafine fibers with ultrafine fibers as the skeleton. The preparation process is green, environmentally friendly, fast and convenient. The ultrafine fiber / aerogel composite material has the characteristics of high strength, heat preservation, noise reduction and scalable preparation, and can be used in the fields of sound-absorbing materials, heat-preserving materials, thermal insulation materials, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 Schematic diagram of the preparation process of the ultrafine fiber / aerogel composite material of the present invention;
[0024] Figure 2 This is a microscopic morphology of the ultrafine fiber / aerogel composite material in Example 1;
[0025] Figure 3 This is an enlarged view of the single fiber microscopic morphology of the ultrafine fiber / aerogel composite material in Example 1. DETAILED DESCRIPTION
[0026] The present invention provides an application of a superfine fiber / aerogel composite material in a sound absorbing material, a heat preservation material or a heat insulating material. The preparation method of the superfine fiber / aerogel composite material comprises the following steps:
[0027] The high-strength hydrogel / ultrafine fiber nonwoven composite material is immersed in water and frozen, and then freeze-dried to obtain the ultrafine fiber / aerogel composite material.
[0028] In the present invention, the method for preparing the high-strength hydrogel / ultrafine fiber nonwoven composite material preferably comprises the following steps:
[0029] (1) melting a first polymer and a second polymer independently to obtain a melt of the first polymer and a melt of the second polymer; and composite spinning the melt of the first polymer and the melt of the second polymer to obtain a water-soluble polyvinyl alcohol bicomponent fiber; wherein the first polymer is thermoplastic polyvinyl alcohol;
[0030] (2) drawing the water-soluble polyvinyl alcohol bicomponent fiber to obtain short fibers;
[0031] (3) combing the short fibers to obtain a polyvinyl alcohol two-component fiber web;
[0032] (4) reinforcing the polyvinyl alcohol two-component fiber web to obtain a water-soluble polyvinyl alcohol two-component carded-needle-punched nonwoven material;
[0033] (5) subjecting the water-soluble polyvinyl alcohol two-component carded-needle-punched nonwoven material to a water-soluble fiber-opening treatment to obtain a solution containing the nonwoven material;
[0034] (6) Mixing the solution containing the nonwoven material and the additive solution, and sequentially performing cross-linking and freezing treatments to obtain the high-strength hydrogel / ultrafine fiber nonwoven composite material.
[0035] In the present invention, the weight average molecular weight of the thermoplastic polyvinyl alcohol in step (1) is preferably 5000-8000, more preferably 6000-7100, more preferably 6500-6700; the alcoholysis degree of the thermoplastic polyvinyl alcohol is preferably 88-99%, more preferably 90-98%, more preferably 92-95%; the polymerization degree of the thermoplastic polyvinyl alcohol is preferably 400-1000, more preferably 500-900, more preferably 600-800; the melt flow index of the thermoplastic polyvinyl alcohol is preferably 25-60 g / 10 min, more preferably 30-46 g / 10 min, more preferably 35-40 g / 10 min.
[0036] In the present invention, the thermoplastic polyvinyl alcohol in step (1) is prepared according to patent CN116876153A.
[0037] In the present invention, the second polymer preferably includes one or more of polyethylene compounds, polypropylene compounds, polyester compounds, polyamide compounds and polylactic acid compounds; polyethylene compounds are preferably polyethylene or polyethylene derivative polymers, polypropylene compounds are preferably polypropylene or polypropylene derivative polymers, polyester compounds are preferably polyesters or polyester derivative polymers, polyamide compounds are preferably polyamides or polyamide derivative polymers, polylactic acid compounds are preferably polylactic acid or polylactic acid derivative polymers. The present invention does not specifically limit the types of the above-mentioned derivative polymers, as long as they can be composite-spun with thermoplastic polyvinyl alcohol.
[0038] In the present invention, the mass fraction of the thermoplastic polyvinyl alcohol in the water-soluble polyvinyl alcohol bicomponent fiber is preferably 10 to 90%, more preferably 20 to 60%, and even more preferably 40 to 50%.
[0039] In the present invention, during the melting process, functional particles such as antistatic agents, light stabilizers, antioxidants, weather stabilizers, antifogging agents, anti-blocking agents, lubricants, nucleating agents, pigments and other additives or other polymers can be added to the two polymer raw materials through conventional selection as needed.
[0040] In the present invention, in step (1), melting and spinning are preferably carried out in a conjugated two-component melt spinning machine, and the first polymer and the second polymer are respectively added to the feed port A and the feed port B, respectively, extruded through the screw A and the screw B, and then metered by a metering pump, and then composite spinning is carried out through a spinning assembly, and the fibers obtained by spinning are bundled to obtain a fiber bundle, and finally wound on a silk drum through a winding device to form a water-soluble polyvinyl alcohol two-component fiber.
[0041] In the present invention, in step (2), the water-soluble polyvinyl alcohol bicomponent fiber wound on the filament drum is unwound and then stretched; the stretching is preferably carried out in a constant temperature stretching box, and the temperature in the entire constant temperature stretching box is kept constant by electric heating, so that the fiber is heated evenly, and the constant temperature stretching box has a multi-stage stretching structure, and the number of stretching rollers is preferably 1 to 6, more preferably 2 to 5, and more preferably 3 to 4.
[0042] In the present invention, the stretching method in step (2) is preferably dry heat stretching, which can avoid the dissolution of the polyvinyl alcohol component; the stretching temperature is preferably 60-120°C, more preferably 70-110°C, and more preferably 80-100°C; the stretching ratio is preferably 2-6 times, more preferably 3-5 times, and more preferably 4-4.5 times. The specific stretching ratio achieves full stretching of the water-soluble polyvinyl alcohol bicomponent fiber; and the mechanical properties of the water-soluble polyvinyl alcohol bicomponent fiber are further improved by stretching.
[0043] In the present invention, after the stretching in step (2) is completed, the obtained sample is cut by a fiber cutter to obtain short fibers; the length of the short fibers is preferably 20 to 60 mm, more preferably 30 to 50 mm, and even more preferably 40 to 45 mm.
[0044] In the present invention, the combing step (3) preferably comprises combing a and combing b performed sequentially, wherein the combing a is performed by high-speed random combing. After the combing a is completed, a fiber web is obtained, and the weight of the fiber web is preferably 50 to 150 g / m 2 , more preferably 80 to 120 g / m 2 , more preferably 100 to 110 g / m 2 The carding method b is parallel laying, full cross laying or half cross laying. After the carding b is completed, a polyvinyl alcohol two-component fiber web is obtained. The weight of the polyvinyl alcohol two-component fiber web is preferably 400 to 1000 g / m 2 , more preferably 500 to 900 g / m 2 , more preferably 600 to 800 g / m 2 .
[0045] In the present invention, the reinforcement method in step (4) is preferably acupuncture, and the density of acupuncture is preferably 500 to 2000 punctures / cm 2 , more preferably 800 to 1500 thorns / cm 2 , more preferably 1000 to 1200 thorns / cm 2 The depth of acupuncture is preferably 4 to 10 mm, more preferably 5 to 9 mm, and more preferably 6 to 8 mm; the frequency of acupuncture is preferably 400 to 2000 times / min, more preferably 800 to 1500 times / min, and more preferably 1200 to 1300 times / min.
[0046] In the present invention, the mass fraction of polyvinyl alcohol in the solution containing the nonwoven material in step (5) is preferably 5 to 60%, more preferably 15 to 35%, and even more preferably 20 to 30%.
[0047] In the present invention, in step (5), the water-soluble polyvinyl alcohol two-component carded-needle-punched nonwoven material is placed in a mold containing water (the water-soluble polyvinyl alcohol two-component carded-needle-punched nonwoven material is the same size as the mold, which can avoid the collapse of the nonwoven material structure after the polyvinyl alcohol is dissolved in water on the one hand, and on the other hand, it is beneficial for the polyvinyl alcohol component to be evenly dispersed in the nonwoven material structure) and subjected to a water-soluble fiber-opening treatment. After the polyvinyl alcohol component is dissolved, the water-soluble fiber-opening treatment is completed to obtain a solution containing the nonwoven material.
[0048] In the present invention, the temperature of the water-soluble fiber-opening treatment is determined according to the alcoholysis degree of the thermoplastic polyvinyl alcohol. When the alcoholysis degree of the thermoplastic polyvinyl alcohol is 88-90%, the temperature of the water-soluble fiber-opening treatment needs to be ≥60°C. When the alcoholysis degree of the thermoplastic polyvinyl alcohol is 90-95% and does not include 90%, the temperature of the water-soluble fiber-opening treatment needs to be ≥80°C. When the alcoholysis degree of the thermoplastic polyvinyl alcohol is 95-99% and does not include 95%, the temperature of the water-soluble fiber-opening treatment needs to be ≥90°C.
[0049] In the present invention, the additive in the additive solution of step (6) preferably includes one or more of sodium tetraborate, glutaraldehyde, sodium sulfate, zinc sulfate, maleic anhydride, phthaloyl chloride, phthalic anhydride, glutaric anhydride, succinic anhydride, phthalic acid, epichlorohydrin, formaldehyde, sodium hydroxide, potassium hydroxide and boric acid; the present invention does not specifically limit the position of the substituent in terephthaloyl chloride, phthalic anhydride and phthalic acid; the mass fraction of the additive solution is preferably 5-20%, more preferably 8-18%, and more preferably 10-16%.
[0050] In the present invention, the mass fraction of the additive in the solution obtained by mixing in step (6) is preferably 1 to 10%, more preferably 3 to 6%, and even more preferably 3.5 to 5%.
[0051] In the present invention, the cross-linking temperature in step (6) is preferably 40-100°C, more preferably 60-90°C, more preferably 70-80°C; the cross-linking time is preferably 1-8h, more preferably 2-5h, more preferably 3-4h.
[0052] In the present invention, after the cross-linking in step (6) is completed, the mold is placed in an ultrasonic instrument for ultrasonic treatment to remove bubbles in the system, and finally a freezing treatment is performed. After the freezing treatment, the solution is in a hydrogel state, that is, a high-strength hydrogel / ultrafine fiber non-woven composite material; the ultrasonic temperature is preferably 50 to 95°C, more preferably 65 to 90°C, and more preferably 75 to 80°C; the ultrasonic time is preferably 1 to 6 hours, more preferably 2 to 5 hours, and more preferably 3 to 4 hours.
[0053] In the present invention, the freezing treatment in step (6) preferably comprises the following steps:
[0054] Freeze at -5 to -25°C for 6 to 12 hours. After freezing, thaw at 5 to 25°C for 2 to 12 hours. Repeat the above process 4 to 8 times to complete the freezing process.
[0055] In the present invention, the freezing treatment in step (6) further preferably comprises the following steps:
[0056] Freeze at -8 to -18°C for 7 to 11 hours. After freezing, thaw at 10 to 20°C for 4 to 10 hours. Repeat the above process 5 to 7 times to complete the freezing process.
[0057] In the present invention, the freezing treatment in step (6) more preferably comprises the following steps:
[0058] Freeze at -10 to -15°C for 8 to 10 hours. After freezing, thaw at 14 to 16°C for 6 to 9 hours. Repeat the above process 6 times to complete the freezing process.
[0059] In the present invention, the high-strength hydrogel / ultrafine fiber nonwoven composite material is immersed in water and frozen to freeze; the freezing environment is preferably a liquid nitrogen environment.
[0060] In the present invention, the ice-block sample obtained by freezing is freeze-dried, and the freeze-drying temperature is preferably -20 to -60°C, more preferably -30 to -50°C, and more preferably -40°C; after freeze-drying until the water is completely removed, the ultrafine fiber / aerogel composite material is obtained.
[0061] The schematic diagram of the preparation process of the ultrafine fiber / aerogel composite material in the present invention is as follows: Figure 1 shown.
[0062] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0063] Example 1
[0064] Thermoplastic polyvinyl alcohol (weight average molecular weight of 6700, alcoholysis degree of 88%, polymerization degree of 500, melt flow index of 40g / 10min) and polyamide are added to feed port A (thermoplastic polyvinyl alcohol) and feed port B (polyamide) respectively, extruded through screw A and screw B respectively, then metered by a metering pump, and then composite spinning is performed through a spinning assembly, the fibers obtained by spinning are bundled to obtain a fiber bundle, and finally wound on a yarn drum through a winding device to form a water-soluble polyvinyl alcohol bicomponent fiber, the cross-sectional structure of which is a hollow orange segment type (8+8), wherein the mass fraction of thermoplastic polyvinyl alcohol in the water-soluble polyvinyl alcohol bicomponent fiber is 50%;
[0065] The water-soluble polyvinyl alcohol bicomponent fiber wound on the filament drum is unwound, and then dry-heat stretched in a constant temperature stretching box. The temperature in the entire constant temperature stretching box is kept constant by electric heating. The stretching temperature is set to 80°C. The constant temperature stretching box has 3 stretching rollers, and the stretching ratio is set to 4 times. After the stretching is completed, the fiber cutter is used to cut it into short fibers of 40 mm.
[0066] The short fibers are randomly combed at high speed to obtain a weight of 80 g / m 2 The fiber web is then fully cross-laid to obtain a gram weight of 500g / m 2 The polyvinyl alcohol bicomponent fiber mesh is then reinforced (needled) by a needle punching machine, and the needle punching density is set to 1000 needles / cm 2 , depth of 8 mm, frequency of 800 times / min, to obtain a water-soluble polyvinyl alcohol two-component carding-needle punching nonwoven material;
[0067] The water-soluble polyvinyl alcohol two-component combed-needle-punched nonwoven material is placed in a mold containing water (the water-soluble polyvinyl alcohol two-component combed-needle-punched nonwoven material has the same size as the mold), and a water-soluble fiber opening treatment is performed at a temperature of 80°C. After the polyvinyl alcohol component is dissolved, the water-soluble fiber opening treatment is completed to obtain a solution containing a nonwoven material (the mass fraction of polyvinyl alcohol in the solution containing the nonwoven material is 20%), and then a glutaraldehyde solution with a mass fraction of 5% is added for mixing, and the mass fraction of glutaraldehyde in the mixed solution is 1%, and cross-linking is performed at 80°C for 4h. After the cross-linking is completed, the mold is placed in an ultrasonic instrument for ultrasonication at 80°C for 6h, and frozen at -10°C for 6h. After the freezing is completed, it is thawed at 20°C for 3h, and the above process is repeated 5 times to obtain a high-strength hydrogel / ultrafine fiber nonwoven composite material;
[0068] The high-strength hydrogel / ultrafine fiber nonwoven composite material is immersed in water and then placed in a liquid nitrogen environment to freeze it; then, the ice-block sample obtained by freezing is placed in a freeze dryer and the temperature is set to -40°C. After the moisture is completely removed, the ultrafine fiber / aerogel composite material is obtained.
[0069] The microscopic morphology of the ultrafine fiber / aerogel composite material in this embodiment is as follows: Figure 2 As shown. Figure 2 It can be seen that in the ultrafine fiber / aerogel composite material, the aerogel formed after the polyvinyl alcohol component is dissolved and cross-linked is evenly filled in the ultrafine fiber nonwoven material, further enlarging the fiber.
[0070] The enlarged microscopic morphology of a single fiber of the ultrafine fiber / aerogel composite material in this embodiment is shown in FIG. Figure 3 As shown. Figure 3 It can be seen that the TPVA component in the composite fiber is dissolved and cross-linked to form a two-component fiber of ultrafine fiber / aerogel. This aerogel is evenly filled in the two-component fiber non-woven material of ultrafine fiber / aerogel. The prepared composite material is extremely beneficial for thermal insulation, sound absorption and heat insulation.
[0071] The diameter of the water-soluble polyvinyl alcohol bicomponent fiber obtained in this example is 24 μm, and the diameter of the ultrafine fiber in the ultrafine fiber / aerogel composite material is 5.6 μm.
[0072] Example 2
[0073] Thermoplastic polyvinyl alcohol (weight average molecular weight of 7100, alcoholysis degree of 98%, polymerization degree of 600, melt flow index of 46g / 10min) and polylactic acid are added to feed port A (thermoplastic polyvinyl alcohol) and feed port B (polylactic acid) respectively, extruded through screw A and screw B respectively, then metered by a metering pump, and then composite spun through a spinning assembly, the spun fibers are bundled to obtain a fiber bundle, and finally wound on a yarn drum through a winding device to form a water-soluble polyvinyl alcohol bicomponent fiber, the cross-sectional structure of which is an island-in-sea type (37 islands), wherein the mass fraction of thermoplastic polyvinyl alcohol in the water-soluble polyvinyl alcohol bicomponent fiber is 40%;
[0074] The water-soluble polyvinyl alcohol bicomponent fiber wound on the filament drum is unwound, and then dry-heat stretched in a constant temperature stretching box. The temperature in the entire constant temperature stretching box is kept constant by electric heating. The stretching temperature is set to 60°C. The constant temperature stretching box has 4 stretching rollers, and the stretching ratio is set to 4.5 times. After the stretching is completed, the fiber cutter is used to cut it into short fibers of 30 mm.
[0075] The short fibers are randomly combed at high speed to obtain a weight of 100 g / m 2The fiber web is semi-cross-laid to obtain a gram weight of 400g / m 2 The polyvinyl alcohol bicomponent fiber mesh is then reinforced (needled) by a needle punching machine, and the needle punching density is set to 800 needles / cm 2 , depth of 6 mm, frequency of 1000 times / min, to obtain a water-soluble polyvinyl alcohol two-component carding-needle punching nonwoven material;
[0076] The water-soluble polyvinyl alcohol two-component carded-needle-punched nonwoven material is placed in a mold containing water (the water-soluble polyvinyl alcohol two-component carded-needle-punched nonwoven material has the same size as the mold), and a water-soluble fiber opening treatment is performed at 90°C. After the polyvinyl alcohol component is dissolved, the water-soluble fiber opening treatment is completed to obtain a solution containing a nonwoven material (the mass fraction of polyvinyl alcohol in the solution containing the nonwoven material is 35%), and then a glutaric anhydride solution with a mass fraction of 8% is added for mixing. The mass fraction of glutaraldehyde in the mixed solution is 3%, and cross-linking is performed at 70°C for 8h. After the cross-linking is completed, the mold is placed in an ultrasonic instrument for ultrasonication at 75°C for 4h, and frozen at -15°C for 8h. After the freezing is completed, it is thawed at 10°C for 6h. The above process is repeated 4 times to obtain a high-strength hydrogel / ultrafine fiber nonwoven composite material;
[0077] The high-strength hydrogel / ultrafine fiber nonwoven composite material is immersed in water and then placed in a liquid nitrogen environment to freeze it; then, the ice-block sample obtained by freezing is placed in a freeze dryer and the temperature is set to -20°C. After the moisture is completely removed, the ultrafine fiber / aerogel composite material is obtained.
[0078] The diameter of the water-soluble polyvinyl alcohol bicomponent fiber obtained in this example is 27 μm, and the diameter of the ultrafine fiber in the ultrafine fiber / aerogel composite material is 3.4 μm.
[0079] Example 3
[0080] Thermoplastic polyvinyl alcohol (weight average molecular weight of 6800, alcoholysis degree of 95%, polymerization degree of 550, melt flow index of 42g / 10min) and polylactic acid are added to feed port A (thermoplastic polyvinyl alcohol) and feed port B (polylactic acid) respectively, extruded through screw A and screw B respectively, then metered by a metering pump, and then composite spinning is performed through a spinning assembly, the fibers obtained by spinning are bundled to obtain a fiber bundle, and finally wound on a yarn drum through a winding device to form a water-soluble polyvinyl alcohol bicomponent fiber, the cross-sectional structure of which is an orange segment type (16+16), wherein the mass fraction of thermoplastic polyvinyl alcohol in the water-soluble polyvinyl alcohol bicomponent fiber is 60%;
[0081] The water-soluble polyvinyl alcohol bicomponent fiber wound on the filament drum is unwound, and then dry-heat stretched in a constant temperature stretching box. The temperature in the entire constant temperature stretching box is kept constant by electric heating. The stretching temperature is set to 80°C. The constant temperature stretching box has 3 stretching rollers, and the stretching ratio is set to 3 times. After the stretching is completed, the fiber cutter is used to cut it into short fibers of 50 mm.
[0082] The short fibers are randomly combed at high speed to obtain a weight of 80 g / m 2 The fiber web is then fully cross-laid to obtain a gram weight of 600g / m 2 The polyvinyl alcohol bicomponent fiber mesh is then reinforced (needled) by a needle punching machine, and the needle punching density is set to 1000 needles / cm 2 , depth of 10 mm, frequency of 1000 times / min, to obtain a water-soluble polyvinyl alcohol two-component carding-needle punching nonwoven material;
[0083] The water-soluble polyvinyl alcohol two-component carded-needle-punched nonwoven material is placed in a mold containing water (the water-soluble polyvinyl alcohol two-component carded-needle-punched nonwoven material has the same size as the mold), and a water-soluble fiber opening treatment is performed at a temperature of 90°C. After the polyvinyl alcohol component is dissolved, the water-soluble fiber opening treatment is completed to obtain a solution containing a nonwoven material (the mass fraction of polyvinyl alcohol in the solution containing the nonwoven material is 30%), and then a 10% mass fraction of phthalic anhydride solution is added for mixing, the mass fraction of glutaraldehyde in the mixed solution is 3.5%, and cross-linking is performed at 60°C for 5h. After the cross-linking is completed, the mold is placed in an ultrasonic instrument and ultrasonicated at 65°C for 5h, and then frozen at -10°C for 6h. After the freezing is completed, it is thawed at 25°C for 3h, and the above process is repeated 6 times to obtain a high-strength hydrogel / ultrafine fiber nonwoven composite material;
[0084] The high-strength hydrogel / ultrafine fiber nonwoven composite material is immersed in water and then placed in a liquid nitrogen environment to freeze it; then, the ice-block sample obtained by freezing is placed in a freeze dryer and the temperature is set to -60°C. After the moisture is completely removed, the ultrafine fiber / aerogel composite material is obtained.
[0085] The diameter of the water-soluble polyvinyl alcohol bicomponent fiber obtained in this example is 22 μm, and the diameter of the ultrafine fiber in the ultrafine fiber / aerogel composite material is 3.1 μm.
[0086] Comparative Example 1
[0087] The polyester and the polyamide are added to the feed port A (polyester) and the feed port B (polyamide) respectively, and extruded through the screw A and the screw B respectively, and then metered by the metering pump, and then composite spinning is performed through the spinning assembly, and the fibers obtained by spinning are bundled to obtain a fiber bundle, and finally wound on the yarn drum through a winding device to form a two-component fiber, and the cross-sectional structure is a hollow orange segment type (8+8), wherein the mass ratio of polyester to polyamide is 5:5;
[0088] The two-component fiber wound on the filament drum is unwound, and then dry-heat drawn in a constant temperature drawing box. The temperature in the entire constant temperature drawing box is kept constant by electric heating. The drawing temperature is set to 80°C. The constant temperature drawing box has a multi-stage drawing structure, and the drawing ratio is set to 4 times. After the drawing is completed, it is cut into short fibers of 40 mm by a fiber cutter.
[0089] The short fibers are randomly combed at high speed to obtain a weight of 80 g / m 2 The fiber web is then fully cross-laid to obtain a gram weight of 500g / m 2 The bicomponent fiber web is then reinforced (needled) by a needle punching machine, and the needle punching density is set to 1000 needles / cm 2 , depth of 8 mm, frequency of 800 times / min, to obtain a two-component needle-punched nonwoven material.
[0090] The properties of the ultrafine fiber / aerogel composite materials obtained in Examples 1 to 3 and the two-component needle-punched nonwoven material obtained in Comparative Example 1 were tested, wherein the tensile strength of the ultrafine fiber / aerogel composite material was tested according to GB / T 24218.3-2010, the thermal conductivity was measured according to GBT 10297-2015, and the sound absorption coefficient was tested according to GB T 18696.2-2002. The performance test results of the ultrafine fiber / aerogel composite materials in Examples 1 to 3 and the two-component needle-punched nonwoven material in Comparative Example 1 were obtained, as shown in Table 1.
[0091] Table 1 Performance test results of the ultrafine fiber / aerogel composite materials in Examples 1 to 3 and the two-component needle-punched nonwoven material in Comparative Example 1
[0092]
[0093] As can be seen from Table 1, the ultrafine fiber / aerogel composite material prepared by the present invention has the characteristics of high strength, heat preservation, noise reduction, etc., and can be used in the fields of sound absorbing materials, heat preservation materials, thermal insulation materials, etc.
[0094] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. Application of an ultrafine fiber / aerogel composite material in a sound absorbing material, a heat preservation material or a heat insulating material, characterized in that: The preparation method of the ultrafine fiber / aerogel composite material comprises the following steps: The high-strength hydrogel / ultrafine fiber nonwoven composite material is immersed in water and frozen, and then freeze-dried to obtain the ultrafine fiber / aerogel composite material.
2. The use of the ultrafine fiber / aerogel composite material according to claim 1 in sound absorbing materials, thermal insulation materials or heat insulating materials, characterized in that: The preparation method of the high-strength hydrogel / ultrafine fiber nonwoven composite material comprises the following steps: (1) melting a first polymer and a second polymer independently to obtain a melt of the first polymer and a melt of the second polymer; and composite spinning the melt of the first polymer and the melt of the second polymer to obtain a water-soluble polyvinyl alcohol bicomponent fiber; The first polymer is thermoplastic polyvinyl alcohol; (2) drawing the water-soluble polyvinyl alcohol bicomponent fiber to obtain short fibers; (3) combing the short fibers to obtain a polyvinyl alcohol two-component fiber web; (4) reinforcing the polyvinyl alcohol two-component fiber web to obtain a water-soluble polyvinyl alcohol two-component carded-needle-punched nonwoven material; (5) subjecting the water-soluble polyvinyl alcohol two-component carded-needle-punched nonwoven material to a water-soluble fiber-opening treatment to obtain a solution containing the nonwoven material; (6) Mixing the solution containing the nonwoven material and the additive solution, and sequentially performing cross-linking and freezing treatments to obtain the high-strength hydrogel / ultrafine fiber nonwoven composite material.
3. The use of the ultrafine fiber / aerogel composite material as claimed in claim 2 in sound absorbing materials, thermal insulation materials or heat insulating materials, characterized in that: The weight average molecular weight of the thermoplastic polyvinyl alcohol in step (1) is 5000-8000, the alcoholysis degree of the thermoplastic polyvinyl alcohol is 88-99%, the polymerization degree of the thermoplastic polyvinyl alcohol is 400-1000, and the melt flow index of the thermoplastic polyvinyl alcohol is 25-60 g / 10 min; The second polymer includes one or more of polyethylene compounds, polypropylene compounds, polyester compounds, polyamide compounds and polylactic acid compounds; The mass fraction of thermoplastic polyvinyl alcohol in the water-soluble polyvinyl alcohol bicomponent fiber is 10-90%.
4. The use of the ultrafine fiber / aerogel composite material as claimed in claim 3 in sound absorbing materials, thermal insulation materials or heat insulating materials, characterized in that: The freezing environment is a liquid nitrogen environment.
5. The use of the ultrafine fiber / aerogel composite material as claimed in claim 4 in sound absorbing materials, thermal insulation materials or heat insulating materials, characterized in that: The freeze-drying temperature is -20 to -60°C.
6. Use of the ultrafine fiber / aerogel composite material according to claim 5 in sound absorbing materials, thermal insulation materials or heat insulating materials, characterized in that: The tensile strength of the ultrafine fiber / aerogel composite material is 10.6-14.0 MPa; the thermal conductivity of the ultrafine fiber / aerogel composite material at 40° C. is 0.04061-0.04357 W·m -1 ·K -1 , the thermal conductivity at 80°C is 0.04531~0.04762W·m -1 ·K -1 The sound absorption coefficient of the ultrafine fiber / aerogel composite material is 0.80-0.84 at 1000HZ, 0.91-0.94 at 2000HZ, and 0.96-0.98 at 4000HZ.
Citation Information
Patent Citations
Orange segment type spunbonded spunlaced superfine fiber non-woven filtering material based on water-soluble splitting and preparation method and application of orange segment type spunbonded spunlaced superfine fiber non-woven filtering material