High-performance automobile bumper material and preparation method thereof
By using components such as PP, carbon nanotubes and EPDM in automotive bumper materials, combined with surface treatment and twin screw extrusion technology, the problem of insufficient impact resistance of existing automobile bumper materials is solved, and the material resistance is significantly improved Impact performance and safety performance.
Patent Information
- Application Number
- CN202411054925.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-12-06
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of bumper materials, and in particular relates to a high-performance automobile bumper material and a preparation method thereof. Background Art
[0002] PP is a semi-crystalline material. It is harder and has a higher melting point than PE. Since homopolymer PP is very brittle below 0°C, many commercial PP materials are random copolymers with 1-4% ethylene or clamp copolymers with higher ethylene content. Copolymer PP materials have lower heat distortion temperature (100°C), low transparency, low gloss, and low rigidity, but have stronger impact strength. The strength of PP increases with the increase of ethylene content. The Vicat softening temperature of PP is 150°C. Due to the high crystallinity, the surface stiffness and scratch resistance of this material are very good. PP does not have environmental stress cracking problems. Usually, PP is modified by adding glass fiber, metal additives or thermoplastic rubber. The flow rate MFR of PP ranges from 1 to 40. Low MFR PP materials have better impact resistance but lower ductility. For materials with the same MFR, the strength of copolymers is higher than that of homopolymers. Due to crystallization, the shrinkage rate of PP is quite high, generally 1.8-2.5%. And the directional uniformity of shrinkage is much better than that of materials such as PE-HD. Adding 30% of glass additives can reduce the shrinkage to 0.7%. Both homopolymer and copolymer PP materials have excellent moisture absorption resistance, acid and alkali corrosion resistance, and solubility resistance. However, it has no resistance to aromatic hydrocarbon solvents, chlorinated hydrocarbon solvents, etc. PP is not as resistant to oxidation at high temperatures as PE. The proportion of PP resin used in injection molded products can account for about half, among which daily necessities use ordinary PP as raw materials, automotive accessories use reinforced or toughened PP as raw materials, and other uses are mainly based on copolymer polypropylene PPC raw materials with high impact strength and low brittle temperature. PP is increasingly becoming the dominant material for automotive accessories and has become the largest automotive plastic variety. Toughened PP is used for bumpers and wheel covers, etc., and reinforced PP is used for dashboards, steering wheels, handles, containers, battery shells, etc. Polypropylene is a non-toxic, odorless, milky white, highly crystalline polymer. It is particularly stable to water, with a water absorption rate of only 0.01% in water. It has good formability, good surface gloss of the product, and is easy to color. Polypropylene has high crystallinity and regular structure, so it has excellent mechanical properties. The absolute value of the mechanical properties of polypropylene is higher than that of polyethylene, but it is still a relatively low variety among plastic materials, and its tensile strength can only reach 30MPa or slightly higher. Polypropylene with a larger isotactic index has a higher tensile strength, but with the increase of the isotactic index, the impact strength of the material decreases, but it does not change after it drops to a certain value. Temperature and loading rate have a great influence on the toughness of polypropylene. When the temperature is higher than the glass transition temperature, the impact damage is a ductile fracture, and below the glass transition temperature is a brittle fracture, and the impact strength value drops significantly. Increasing the loading rate can increase the temperature at which the ductile fracture turns into a brittle fracture. Polypropylene has excellent resistance to bending fatigue, and its products can be bent 106 times at room temperature without damage.Polypropylene has good heat resistance. The products can be sterilized at a temperature above 100℃. Under the condition of no external force, it will not deform at 150℃. The brittle temperature is -35℃. It will embrittle below -35℃. Polypropylene has good chemical stability. Except for being corroded by concentrated sulfuric acid and concentrated nitric acid, it is relatively stable to various other chemical reagents. However, low molecular weight aliphatic hydrocarbons, aromatic hydrocarbons and chlorinated hydrocarbons can soften and swell polypropylene. At the same time, its chemical stability is improved with the increase of crystallinity. Therefore, polypropylene is suitable for making various chemical pipelines and accessories, and has good anti-corrosion effect. Polypropylene is very sensitive to ultraviolet rays. Adding zinc oxide, dilauryl thiodipropionate, carbon black or similar milky white fillers can improve its aging resistance. At present, most of the materials used for bumpers have problems such as poor shrinkage control, low paint adhesion, poor weather resistance, poor toughness, unsatisfactory impact resistance, small elongation at break and low heat deformation temperature. Chinese invention patent application CN1566196A discloses a novel polypropylene composite material, which is composed of the following components in parts by weight: 25-60 parts of copolymerized polypropylene granules, 5-20 parts of thermoplastic elastomer, 0-20 parts of high-density polyethylene, 0-40 parts of mineral filler, 0-10 parts of polar polymer material, 0.1-0.6 parts of thermal oxidation inhibitor, 0.1-0.3 parts of coupling agent, and 0.1-0.3 parts of light stabilizer. The composite material has extremely strong adhesion, but the volume change of the material is large and the impact resistance is poor; the fluidity during molding is poor and the preparation process is complicated. Chinese invention patent CN1235989A discloses a paintable modified polypropylene composition, which comprises 100 parts of polypropylene, 10 to 50 parts of rubber-type toughening agent, 5 to 15 parts of oligomer, 5 to 20 parts of grafted modified polypropylene, and 1 to 15 parts of inorganic filler. The composition is prepared by uniformly mixing the above materials in proportion, extruding and granulating at a processing temperature of 180 to 220°C, and then melt blending; the composition prepared by the above method has an impact strength of up to 629.6 J / m. When used as a material for preparing automobile bumpers, its impact resistance is not high enough and cannot absorb more impact energy, thereby reducing the safety performance of the automobile. Summary of the invention
[0003] In view of this, the technical problem to be solved by the present invention is to provide a high-performance automobile bumper material to avoid the problem of insufficient impact resistance of conventional bumper materials.
[0004] In order to solve the above technical problems, the present invention discloses a high-performance automobile bumper material, comprising 50-100 parts of PP, 30-65 parts of carbon nanotubes, 10-30 parts of EPDM, 1-8 parts of talcum powder, 1-4 parts of antistatic agent, 1-4 parts of antioxidant, 4-10 parts of dispersant, 1-5 parts of plasticizer, and 1-5 parts of ultraviolet absorber.
[0005] According to one embodiment of the present invention, the above-mentioned automobile bumper material includes 50 parts of PP, 30 parts of carbon nanotubes, 10 parts of EPDM, 2 parts of talcum powder, 1 part of antistatic agent, 1 part of antioxidant, 4 parts of dispersant, 1 part of plasticizer, and 1 part of ultraviolet absorber.
[0006] According to one embodiment of the present invention, the above-mentioned automobile bumper material includes 100 parts of PP, 65 parts of carbon nanotubes, 30 parts of EPDM, 8 parts of talcum powder, 4 parts of antistatic agent, 4 parts of antioxidant, 10 parts of dispersant, 5 parts of plasticizer, and 5 parts of ultraviolet absorber.
[0007] According to one embodiment of the present invention, the above-mentioned automobile bumper material includes 80 parts of PP, 45 parts of carbon nanotubes, 20 parts of EPDM, 5 parts of talcum powder, 3 parts of antistatic agent, 3 parts of antioxidant, 6 parts of dispersant, 3 parts of plasticizer, and 3 parts of ultraviolet absorber.
[0008] The present invention also discloses a method for preparing a high-performance automobile bumper material, comprising: Step a. Mixing a 15%-20% aqueous solution of r-aminopropyltriethoxysilane with carbon nanotubes in a ratio of 45:20, heating to 50-80°C, stirring for 30-120min, and then filtering to obtain carbon nanotubes surface-treated with r-aminopropyltriethoxysilane; Step b. Weigh a predetermined number of PP, surface-treated carbon nanotubes, and EPDM into a reactor, inject deionized water, keep the temperature at 70°C for 30 minutes, start stirring at 150 r / min, heat the temperature in the reactor from 70°C to 210°C within 90 minutes, and start timing for 120 minutes after the pressure in the reactor rises to 1.8-2.0MPa, then start depressurization, so that the pressure in the reactor drops to normal pressure after 30 minutes, then heat it to 230°C and keep it warm for 30 minutes; slowly open the vacuum system to gradually reduce the pressure in the reactor to -0.05MPa, keep it for 30 minutes, then discharge the material and cool it; Step c. pelletizing the cooled material, extracting and drying it, and then feeding it into a twin-screw extruder together with talcum powder, antistatic agent, antioxidant, dispersant, plasticizer, and ultraviolet absorber to extrude a bumper material product.
[0009] Compared with the prior art, the present invention can achieve the following technical effects: The bumper material is prepared by mixing PP, carbon nanotubes, EPDM as the main materials and various auxiliary agents to ensure the strength requirements. At the same time, the carbon nanotubes are surface treated to make them stronger.
[0010] Of course, any product implementing the present invention does not necessarily need to achieve all of the above-mentioned technical effects at the same time. DETAILED DESCRIPTION
[0011] The following will describe the implementation methods of the present invention in detail with reference to examples, so that the implementation process of how the present invention applies technical means to solve technical problems and achieve technical effects can be fully understood and implemented accordingly.
[0012] The invention discloses a high-performance automobile bumper material, which comprises 50-100 parts of PP, 30-65 parts of carbon nanotubes, 10-30 parts of EPDM, 1-8 parts of talcum powder, 1-4 parts of antistatic agent, 1-4 parts of antioxidant, 4-10 parts of dispersant, 1-5 parts of plasticizer and 1-5 parts of ultraviolet absorber.
[0013] Example 1. The automobile bumper material includes 50 parts of PP, 30 parts of carbon nanotubes, 10 parts of EPDM, 2 parts of talcum powder, 1 part of antistatic agent, 1 part of antioxidant, 4 parts of dispersant, 1 part of plasticizer, and 1 part of ultraviolet absorber.
[0014] Step a. Mixing a 15%-20% aqueous solution of r-aminopropyltriethoxysilane with carbon nanotubes in a ratio of 45:20, heating to 50-80°C, stirring for 30-120min, and then filtering to obtain carbon nanotubes surface-treated with r-aminopropyltriethoxysilane; Step b. Weigh the above-mentioned portions of PP, surface-treated carbon nanotubes, and EPDM into a reactor, inject deionized water, keep warm at 70°C for 30 minutes, start stirring at 150 r / min, heat the reactor temperature from 70°C to 210°C within 90 minutes, and start timing for 120 minutes after the pressure in the reactor rises to 1.8-2.0MPa, then start depressurization, so that the pressure in the reactor drops to normal pressure after 30 minutes, and then heat to 230°C and keep warm for 30 minutes; slowly open the vacuum system to gradually reduce the pressure in the reactor to -0.05MPa, keep it for 30 minutes, and then discharge the material for cooling; Step c. pelletizing the cooled material, extracting and drying it, and then feeding it into a twin-screw extruder together with talcum powder, antistatic agent, antioxidant, dispersant, plasticizer, and ultraviolet absorber to extrude a bumper material product.
[0015] Example 2. The automobile bumper material includes 100 parts of PP, 65 parts of carbon nanotubes, 30 parts of EPDM, 8 parts of talcum powder, 4 parts of antistatic agent, 4 parts of antioxidant, 10 parts of dispersant, 5 parts of plasticizer, and 5 parts of ultraviolet absorber.
[0016] Step a. Mixing a 15%-20% aqueous solution of r-aminopropyltriethoxysilane with carbon nanotubes in a ratio of 45:20, heating to 50-80°C, stirring for 30-120min, and then filtering to obtain carbon nanotubes surface-treated with r-aminopropyltriethoxysilane; Step b. Weigh the above-mentioned portions of PP, surface-treated carbon nanotubes, and EPDM into a reactor, inject deionized water, keep warm at 70°C for 30 minutes, start stirring at 150 r / min, heat the reactor temperature from 70°C to 210°C within 90 minutes, and start timing for 120 minutes after the pressure in the reactor rises to 1.8-2.0MPa, then start depressurization, so that the pressure in the reactor drops to normal pressure after 30 minutes, and then heat to 230°C and keep warm for 30 minutes; slowly open the vacuum system to gradually reduce the pressure in the reactor to -0.05MPa, keep it for 30 minutes, and then discharge the material for cooling; Step c. pelletizing the cooled material, extracting and drying it, and then feeding it into a twin-screw extruder together with talcum powder, antistatic agent, antioxidant, dispersant, plasticizer, and ultraviolet absorber to extrude a bumper material product.
[0017] Example 3. The automobile bumper material includes 80 parts of PP, 45 parts of carbon nanotubes, 20 parts of EPDM, 5 parts of talcum powder, 3 parts of antistatic agent, 3 parts of antioxidant, 6 parts of dispersant, 3 parts of plasticizer, and 3 parts of ultraviolet absorber.
[0018] Step a. Mixing a 15%-20% aqueous solution of r-aminopropyltriethoxysilane with carbon nanotubes in a ratio of 45:20, heating to 50-80°C, stirring for 30-120min, and then filtering to obtain carbon nanotubes surface-treated with r-aminopropyltriethoxysilane; Step b. Weigh the above-mentioned portions of PP, surface-treated carbon nanotubes, and EPDM into a reactor, inject deionized water, keep warm at 70°C for 30 minutes, start stirring at 150 r / min, heat the reactor temperature from 70°C to 210°C within 90 minutes, and start timing for 120 minutes after the pressure in the reactor rises to 1.8-2.0MPa, then start depressurization, so that the pressure in the reactor drops to normal pressure after 30 minutes, and then heat to 230°C and keep warm for 30 minutes; slowly open the vacuum system to gradually reduce the pressure in the reactor to -0.05MPa, keep it for 30 minutes, and then discharge the material for cooling; Step c. pelletizing the cooled material, extracting and drying it, and then feeding it into a twin-screw extruder together with talcum powder, antistatic agent, antioxidant, dispersant, plasticizer, and ultraviolet absorber to extrude a bumper material product.
[0019] Example 4. The automobile bumper material includes 80 parts of PP, 20 parts of EPDM, 5 parts of talcum powder, 3 parts of antistatic agent, 3 parts of antioxidant, 6 parts of dispersant, 3 parts of plasticizer, and 3 parts of ultraviolet absorber.
[0020] Step a. Weigh the above-mentioned portions of PP and EPDM and put them into a reactor, inject deionized water, keep the temperature at 70°C for 30 minutes, start stirring at 150 r / min, heat the temperature in the reactor from 70°C to 210°C within 90 minutes, and start timing for 120 minutes after the pressure in the reactor rises to 1.8-2.0MPa, then start pressure relief, so that the pressure in the reactor drops to normal pressure after 30 minutes, then heat it to 230°C and keep it warm for 30 minutes; slowly open the vacuum system to gradually reduce the pressure in the reactor to -0.05MPa, keep it for 30 minutes, then discharge the material and cool it; Step b. pelletizing the cooled material, extracting and drying it, and then feeding it into a twin-screw extruder with talcum powder, an antistatic agent, an antioxidant, a dispersant, a plasticizer, and an ultraviolet absorber to extrude a bumper material product.
[0021] The bumper material products of the above four embodiments were respectively injection molded into finished bumpers of uniform specifications, and then subjected to bumper strength tests. The bumper tests were conducted at a speed of 9.7 km / h for frontal and rear-end collisions with obstacles in the shape of vehicle bumpers, and at a speed of 4.8 km / h for collisions with the front and rear corners of obstacles. It was found that the bumper material of embodiment 3 had the lowest damage and the highest strength, while the bumper material of embodiment 4 had the greatest damage and the weakest strength.
[0022] In summary, the present invention prepares the bumper material by mixing PP, carbon nanotubes, EPDM as main materials and various auxiliary agents to ensure strength requirements. At the same time, the carbon nanotubes are surface treated to have higher strength.
[0023] The above description shows and describes several preferred embodiments of the present invention, but as mentioned above, it should be understood that the present invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the invention concept described herein through the above teachings or the technology or knowledge of the relevant field. Changes and variations made by those skilled in the art do not depart from the spirit and scope of the present invention, and should be within the scope of protection of the claims attached to the present invention.
Claims
1. A high-performance automobile bumper material, characterized in that: include: 50-100 parts of PP, 30-65 parts of carbon nanotubes, 10-30 parts of EPDM, 1-8 parts of talc, 1-4 parts of antistatic agent, 1-4 parts of antioxidant, 4-10 parts of dispersant, 1-5 parts of plasticizer, 1-5 parts of ultraviolet absorber.
2. The high performance automobile bumper material according to claim 1, characterized in that: include: 50 parts of PP, 30 parts of carbon nanotubes, 10 parts of EPDM, 2 parts of talc, 1 part of antistatic agent, 1 part of antioxidant, 4 parts of dispersant, 1 part of plasticizer, and 1 part of ultraviolet absorber.
3. The high performance automobile bumper material according to claim 1, characterized in that: include: 100 parts of PP, 65 parts of carbon nanotubes, 30 parts of EPDM, 8 parts of talc, 4 parts of antistatic agent, 4 parts of antioxidant, 10 parts of dispersant, 5 parts of plasticizer, and 5 parts of ultraviolet absorber.
4. The high performance automobile bumper material according to claim 1, characterized in that: include: 80 parts of PP, 45 parts of carbon nanotubes, 20 parts of EPDM, 5 parts of talc, 3 parts of antistatic agent, 3 parts of antioxidant, 6 parts of dispersant, 3 parts of plasticizer, and 3 parts of ultraviolet absorber.
5. A method for preparing the high-performance automobile bumper material according to claim 1, characterized in that: include: Step a. Mixing a 15%-20% aqueous solution of r-aminopropyltriethoxysilane with carbon nanotubes in a ratio of 45:20, heating to 50-80°C, stirring for 30-120min, and then filtering to obtain carbon nanotubes surface-treated with r-aminopropyltriethoxysilane; Step b. Weigh a predetermined number of PP, surface-treated carbon nanotubes, and EPDM into a reactor, inject deionized water, keep the temperature at 70°C for 30 minutes, start stirring at 150 r / min, heat the temperature in the reactor from 70°C to 210°C within 90 minutes, and start timing for 120 minutes after the pressure in the reactor rises to 1.8-2.0MPa, then start depressurization, so that the pressure in the reactor drops to normal pressure after 30 minutes, then heat it to 230°C and keep it warm for 30 minutes; slowly open the vacuum system to gradually reduce the pressure in the reactor to -0.05MPa, keep it for 30 minutes, then discharge the material and cool it; Step c. pelletizing the cooled material, extracting and drying it, and then feeding it into a twin-screw extruder together with talcum powder, antistatic agent, antioxidant, dispersant, plasticizer, and ultraviolet absorber to extrude a bumper material product.
Citation Information
Patent Citations
Polypropylene composition for coating
CN1235989A
Polypropylene composite materials
CN1566196A
Cited By
High-corrosion-resistance plastic and preparation method thereof
CN120623638A