Preparation method of flame-retardant ethylene-propylene-diene monomer halogen-free elastic rubber material

By combining modified micron-scale magnesium hydroxide powder and homemade carbon black, combined with aminosilane and double-bond silane coupling agent, the problems of combustion easiness and smoke generation of ethylene propylene rubber materials are solved, achieving efficient resistance The balance of combustion and mechanical properties.

CN119081301APending Publication Date: 2024-12-06ZHENJIANG HUA NUCLEAR EQUIP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411393877.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-08
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing ethylene propylene rubber materials have problems with combustion ease and smoke generation in vehicle sealing strips, making it difficult to take into account both flame retardant properties, mechanical properties and extrusion processing properties.

Method used

Modified micron-scale magnesium hydroxide powder and homemade carbon black are treated with aminosilane and polyborosiloxane, and the carbon black is treated with double bond silane coupling agent to enhance the tensile strength and mechanical properties of the material. The ceramic-type carbon layer is formed during combustion by grafting silicone to enhance the flame retardant effect.

Benefits of technology

It improves the tensile strength and extrusion processing properties of the material, while significantly enhancing the flame retardant performance, balancing the mechanical properties and processing properties, and reducing smoke generation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005073180260000021
    Figure BDA0005073180260000021
  • Figure BDA0005073180260000111
    Figure BDA0005073180260000111
  • Figure FDA0005073180250000011
    Figure FDA0005073180250000011
Patent Text Reader

Abstract

The invention discloses a preparation method of a flame-retardant ethylene-propylene-diene monomer halogen-free elastic rubber material, and relates to the technical field of high polymer materials. The preparation method comprises the following steps: taking raw materials in parts by weight, plastifying ethylene propylene diene monomer for 5-8 times, sequentially feeding zinc oxide, sodium stearate, an accelerant EG-3, a flame-retardant system, self-made carbon black, a plasticizer, sulfur and a charring agent, mixing, carrying out thin-passing on the mixed rubber for 6-10 times, discharging sheets, putting the discharged rubber sheets into a mold, heating, pressurizing and vulcanizing, and carrying out high-temperature vulcanization, so as to obtain the flame-retardant ethylene propylene diene monomer rubber. The flame-retardant ethylene-propylene-diene monomer halogen-free elastic rubber material is obtained. The product prepared by the invention has excellent flame retardant property, mechanical property and extrusion processability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a method for preparing a flame-retardant ethylene propylene diene monomer halogen-free elastic rubber material. Background Art

[0002] The molecular chain of EPDM is flexible and elastic. Its macromolecular side chain contains a small amount of double bonds, which provide reactive sites for sulfur vulcanization. Compared with general-purpose rubbers such as NR, SBR and CR, EPDM has particularly excellent weather resistance, ozone resistance, UV resistance and hot air aging resistance. Therefore, it is widely used in door and window sealing strips of various vehicles such as automobiles, subways and high-speed trains. It has good sealing performance and long service life in long-term use. With the improvement of people's requirements for vehicle safety and comfort, it is not only required that the vehicle door and window sealing strips have excellent sealing performance, but also must have good flame retardant properties and low smoke generation, which is particularly important for subway trains to reduce property losses and casualties caused by fire. However, EPDM is a hydrocarbon chain rubber, which is very easy to burn (limiting oxygen index LOI is about 18), and produces a lot of black smoke when burning. Window sealing strips are generally produced by continuous extrusion microwave high-temperature vulcanization process, which requires EPDM to have excellent extrusion processing performance. The traditional effective flame retardant method is to add halogen-antimony system: small amount of addition, excellent flame retardant performance, small loss of mechanical properties and processing performance, but high toxicity. Another method is to add a large amount of micron hydroxide, but it is difficult to balance the extrusion processing performance and mechanical properties. In order to take into account the flame retardant properties, mechanical properties and extrusion processing performance, it is urgent to develop a flame retardant EPDM halogen-free elastic rubber material. Summary of the invention

[0003] The object of the present invention is to provide a method for preparing a flame retardant EPDM halogen-free elastic rubber material to solve the problems raised in the above background technology.

[0004] To achieve the above object, the present invention provides the following technical solutions:

[0005] A method for preparing a flame-retardant EPDM halogen-free elastic rubber material comprises the following preparation steps:

[0006] (1) Take the raw materials by weight;

[0007] (2) Plasticize the EPDM rubber for 5-8 times, and then add zinc oxide, sodium stearate, accelerator EG-3, flame retardant system, homemade carbon black, plasticizer, sulfur and carbonizing agent in order for mixing;

[0008] (3) Pass the mixed rubber through 6-10 times and make sheets;

[0009] (4) The film is placed in a mold and heated and pressurized for vulcanization to obtain a flame-retardant EPDM halogen-free elastic rubber material.

[0010] Preferably, the weight proportions of the raw materials in step (1) are:

[0011]

[0012] Preferably, the flame retardant system in step (2) is modified micron-sized magnesium hydroxide powder.

[0013] Preferably, the preparation method of the modified micron-sized magnesium hydroxide powder is as follows: the magnesium hydroxide powder is mixed with water in a mass ratio of 1:10-1:20 to form a slurry with a mass fraction of 5-7%, and then the mixture is heated to 40-45° C. and mixed in a constant temperature water bath, the stirring speed is adjusted to 600-800 r / min, and 0.1-0.2 times the mass of the magnesium hydroxide powder and 0.2-0.3 times the mass of the magnesium hydroxide powder are added dropwise. The mixture is mixed for 1-2 hours, filtered and washed, and finally dried in a vacuum drying oven at 60-65° C., followed by grinding to obtain the modified micron-sized magnesium hydroxide powder.

[0014] Preferably, the method for preparing the homemade carbon black in step (2) is:

[0015] Mix carbon black and water in a mass ratio of 1:10-1:20, then heat to 60-75°C and mix in a constant temperature water bath, adjust the stirring speed to 600-800r / min, add 0.2-0.3 times the mass of carbon black double bond silane coupling agent dropwise, mix for 1-2h, filter and wash, and finally dry in a vacuum drying oven at 60-65°C, followed by grinding to obtain homemade carbon black.

[0016] Preferably, the carbon-forming agent in step (2) is prepared by mixing silicone rubber, borate, zinc stannate and organic clay in a mass ratio of 1:2:1:3.

[0017] Preferably, the plasticizer in step (2) is prepared by mixing paraffin oil and dioctyl phthalate in a mass ratio of 2:5.

[0018] Preferably, the vulcanization conditions in step (4) are 22-26 MPa, the temperature is 170-175° C., and the time is 10-15 min.

[0019] In summary, due to the adoption of the above technology, the beneficial effects of the present invention are:

[0020] The present invention utilizes aminosilane and polyborosiloxane to process micron-sized magnesium hydroxide, so that the tensile strength and extrusion processing performance of the composite material are improved. At the same time, the grafted siloxane can migrate to the surface when the polymer system burns to form a ceramic carbon layer to protect the matrix, thereby enhancing the flame retardant effect. Secondly, the reinforcing effect of carbon black is better than that of nano magnesium hydroxide. Adding stearic acid-modified nano magnesium hydroxide will lead to a decrease in the strength of the material. This is because stearic acid-modified nano magnesium hydroxide may improve its dispersion, but weaken the filler-rubber interface effect. Therefore, a double-bond silane coupling agent is used to treat carbon black to increase the interface bonding strength between the carbon black surface and the matrix, and the filler-filled polymer, the filler dispersibility and the filler-polymer interface effect are improved, thereby further improving the mechanical properties of the material. DETAILED DESCRIPTION

[0021] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work belong to the scope of protection of the present invention. Therefore, the following detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but merely represents the selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work belong to the scope of protection of the present invention.

[0022] Example 1

[0023] A method for preparing a flame-retardant EPDM halogen-free elastic rubber material comprises the following preparation steps:

[0024] (1) Take, by weight, 130 parts of EPDM rubber, 8 parts of zinc oxide, 3 parts of sodium stearate, 3 parts of accelerator EG-3, 150 parts of flame retardant system, 60 parts of homemade carbon black, 50 parts of plasticizer, 8 parts of sulfur and 5 parts of carbonizing agent;

[0025] (2) Plasticize the EPDM rubber for 5 times, and add zinc oxide, sodium stearate, accelerator EG-3, flame retardant system, homemade carbon black, plasticizer, sulfur and carbonizing agent in order to mix;

[0026] (3) Pass the mixed rubber through 10 times and make sheets;

[0027] (4) The film is placed in a mold and heated and pressurized for vulcanization to obtain a flame-retardant EPDM halogen-free elastic rubber material.

[0028] The flame retardant system in step (2) is modified micron-sized magnesium hydroxide powder.

[0029] The preparation method of the modified micron-sized magnesium hydroxide powder is as follows: magnesium hydroxide powder and water are mixed in a mass ratio of 1:10 to form a slurry with a mass fraction of 7%, and then the mixture is heated to 40° C. and mixed in a constant temperature water bath, the stirring speed is adjusted to 800 r / min, aminosilane with an amount of 0.2 times the mass of the magnesium hydroxide powder and polyborosiloxane with an amount of 0.3 times the mass of the magnesium hydroxide powder are added dropwise, the mixture is mixed for 1 hour, filtered and washed, and finally dried in a vacuum drying oven at 65° C., followed by grinding to obtain the modified micron-sized magnesium hydroxide powder.

[0030] The preparation method of the homemade carbon black in step (2) is:

[0031] Carbon black and water were mixed in a mass ratio of 1:20, then heated to 60°C and mixed in a constant temperature water bath, the stirring speed was adjusted to 600 r / min, and a double bond silane coupling agent of 0.3 times the mass of the carbon black was added dropwise, mixed for 2 h, filtered and washed, and finally dried in a vacuum drying oven at 60°C, followed by grinding to obtain homemade carbon black.

[0032] The carbon-forming agent in step (2) is prepared by mixing silicone rubber, borate, zinc stannate and organic clay in a mass ratio of 1:2:1:3.

[0033] The plasticizer in step (2) is prepared by mixing paraffin oil and dioctyl phthalate in a mass ratio of 2:5.

[0034] The vulcanization conditions in step (4) are 26 MPa, 175° C., and 10 min.

[0035] Example 2

[0036] A method for preparing a flame-retardant EPDM halogen-free elastic rubber material comprises the following preparation steps:

[0037] (1) Take, by weight, 100 parts of EPDM rubber, 8 parts of zinc oxide, 3 parts of sodium stearate, 5 parts of accelerator EG-3, 150 parts of flame retardant system, 60 parts of homemade carbon black, 60 parts of plasticizer, 8 parts of sulfur and 5 parts of carbonizing agent;

[0038] (2) Plasticize the EPDM rubber for 8 times, and add zinc oxide, sodium stearate, accelerator EG-3, flame retardant system, homemade carbon black, plasticizer, sulfur and carbonizing agent in order for mixing;

[0039] (3) Pass the mixed rubber through 9 times and make sheets;

[0040] (4) The film is placed in a mold and heated and pressurized for vulcanization to obtain a flame-retardant EPDM halogen-free elastic rubber material.

[0041] The flame retardant system in step (2) is modified micron-sized magnesium hydroxide powder.

[0042] The preparation method of the modified micron-sized magnesium hydroxide powder is as follows: magnesium hydroxide powder and water are mixed at a mass ratio of 1:20 to form a slurry with a mass fraction of 5%, and then the mixture is heated to 40° C. and mixed in a constant temperature water bath, the stirring speed is adjusted to 800 r / min, aminosilane with an amount of 0.1 times the mass of the magnesium hydroxide powder and polyborosiloxane with an amount of 0.3 times the mass of the magnesium hydroxide powder are added dropwise, the mixture is mixed for 1 hour, filtered and washed, and finally dried in a vacuum drying oven at 65° C., followed by grinding to obtain the modified micron-sized magnesium hydroxide powder.

[0043] The preparation method of the homemade carbon black in step (2) is:

[0044] Carbon black and water were mixed in a mass ratio of 1:10, then heated to 65°C and mixed in a constant temperature water bath, the stirring speed was adjusted to 700r / min, and a double bond silane coupling agent of 0.2 times the mass of carbon black was added dropwise, mixed for 2h, filtered and washed, and finally dried in a vacuum drying oven at 60°C, followed by grinding to obtain homemade carbon black.

[0045] The carbon-forming agent in step (2) is prepared by mixing silicone rubber, borate, zinc stannate and organic clay in a mass ratio of 1:2:1:3.

[0046] The plasticizer in step (2) is prepared by mixing paraffin oil and dioctyl phthalate in a mass ratio of 2:5.

[0047] The vulcanization conditions in step (4) are 26 MPa, temperature 1705°C, and time 15 min.

[0048] Example 3

[0049] A method for preparing a flame-retardant EPDM halogen-free elastic rubber material comprises the following preparation steps:

[0050] (1) Take, by weight, 100 parts of EPDM rubber, 8 parts of zinc oxide, 2 parts of sodium stearate, 5 parts of accelerator EG-3, 150 parts of flame retardant system, 30 parts of homemade carbon black, 60 parts of plasticizer, 8 parts of sulfur and 10 parts of carbonizing agent;

[0051] (2) Plasticize the EPDM rubber for 6 times, and add zinc oxide, sodium stearate, accelerator EG-3, flame retardant system, homemade carbon black, plasticizer, sulfur and carbonizing agent in order to mix;

[0052] (3) Pass the mixed rubber through 6 times and make sheets;

[0053] (4) The film is placed in a mold and heated and pressurized for vulcanization to obtain a flame-retardant EPDM halogen-free elastic rubber material.

[0054] The flame retardant system in step (2) is modified micron-sized magnesium hydroxide powder.

[0055] The preparation method of the modified micron-sized magnesium hydroxide powder is as follows: magnesium hydroxide powder and water are mixed in a mass ratio of 1:10 to prepare a slurry with a mass fraction of 6%, and then the mixture is heated to 40° C. and mixed in a constant temperature water bath, the stirring speed is adjusted to 800 r / min, aminosilane with an amount of 0.1 times the mass of the magnesium hydroxide powder and polyborosiloxane with an amount of 0.3 times the mass of the magnesium hydroxide powder are added dropwise, the mixture is mixed for 2 hours, filtered and washed, and finally dried in a vacuum drying oven at 65° C., followed by grinding to obtain the modified micron-sized magnesium hydroxide powder.

[0056] The preparation method of the homemade carbon black in step (2) is:

[0057] Carbon black and water were mixed in a mass ratio of 1:10, then heated to 75°C and mixed in a constant temperature water bath, the stirring speed was adjusted to 800r / min, and a double bond silane coupling agent of 0.2 times the mass of carbon black was added dropwise, mixed for 2h, filtered and washed, and finally dried in a vacuum drying oven at 60°C, followed by grinding to obtain homemade carbon black.

[0058] The carbon-forming agent in step (2) is prepared by mixing silicone rubber, borate, zinc stannate and organic clay in a mass ratio of 1:2:1:3.

[0059] The plasticizer in step (2) is prepared by mixing paraffin oil and dioctyl phthalate in a mass ratio of 2:5.

[0060] The vulcanization conditions in step (4) are 23 MPa, 175° C., and 10 min.

[0061] Comparative Example 1

[0062] A method for preparing a flame-retardant EPDM halogen-free elastic rubber material comprises the following preparation steps:

[0063] (1) Take, by weight, 100 parts of EPDM rubber, 8 parts of zinc oxide, 2 parts of sodium stearate, 5 parts of accelerator EG-3, 150 parts of flame retardant system, 30 parts of carbon black, 60 parts of plasticizer, 8 parts of sulfur and 10 parts of carbonizing agent;

[0064] (2) Plasticize the EPDM rubber for 6 times, and add zinc oxide, sodium stearate, accelerator EG-3, flame retardant system, homemade carbon black, plasticizer, sulfur and carbonizing agent in order to mix;

[0065] (3) Pass the mixed rubber through 6 times and make sheets;

[0066] (4) The film is placed in a mold and heated and pressurized for vulcanization to obtain a flame-retardant EPDM halogen-free elastic rubber material.

[0067] The flame retardant system in step (2) is modified micron-sized magnesium hydroxide powder.

[0068] The preparation method of the modified micron-sized magnesium hydroxide powder is as follows: magnesium hydroxide powder and water are mixed in a mass ratio of 1:10 to prepare a slurry with a mass fraction of 6%, and then the mixture is heated to 40° C. and mixed in a constant temperature water bath, the stirring speed is adjusted to 800 r / min, aminosilane with an amount of 0.1 times the mass of the magnesium hydroxide powder and polyborosiloxane with an amount of 0.3 times the mass of the magnesium hydroxide powder are added dropwise, the mixture is mixed for 2 hours, filtered and washed, and finally dried in a vacuum drying oven at 65° C., followed by grinding to obtain the modified micron-sized magnesium hydroxide powder.

[0069] The carbon-forming agent in step (2) is prepared by mixing silicone rubber, borate, zinc stannate and organic clay in a mass ratio of 1:2:1:3.

[0070] The plasticizer in step (2) is prepared by mixing paraffin oil and dioctyl phthalate in a mass ratio of 2:5.

[0071] The vulcanization conditions in step (4) are 23 MPa, 175° C., and 10 min.

[0072] Comparative Example 2

[0073] A method for preparing a flame-retardant EPDM halogen-free elastic rubber material comprises the following preparation steps:

[0074] (1) Take, by weight, 100 parts of EPDM rubber, 8 parts of zinc oxide, 2 parts of sodium stearate, 5 parts of accelerator EG-3, 150 parts of flame retardant system, 30 parts of homemade carbon black, 60 parts of plasticizer, 8 parts of sulfur and 10 parts of carbonizing agent;

[0075] (2) Plasticize the EPDM rubber for 6 times, and add zinc oxide, sodium stearate, accelerator EG-3, flame retardant system, homemade carbon black, plasticizer, sulfur and carbonizing agent in order to mix;

[0076] (3) Pass the mixed rubber through 6 times and make sheets;

[0077] (4) The film is placed in a mold and heated and pressurized for vulcanization to obtain a flame-retardant EPDM halogen-free elastic rubber material.

[0078] The flame retardant system of step (2) is magnesium hydroxide powder.

[0079] The preparation method of the homemade carbon black in step (2) is:

[0080] Carbon black and water were mixed in a mass ratio of 1:10, then heated to 75°C and mixed in a constant temperature water bath, the stirring speed was adjusted to 800r / min, and a double bond silane coupling agent of 0.2 times the mass of carbon black was added dropwise, mixed for 2h, filtered and washed, and finally dried in a vacuum drying oven at 60°C, followed by grinding to obtain homemade carbon black.

[0081] The carbon-forming agent in step (2) is prepared by mixing silicone rubber, borate, zinc stannate and organic clay in a mass ratio of 1:2:1:3.

[0082] The plasticizer in step (2) is prepared by mixing paraffin oil and dioctyl phthalate in a mass ratio of 2:5.

[0083] The vulcanization conditions in step (4) are 23 MPa, 175° C., and 10 min.

[0084] Detection:

[0085] (1) Mechanical properties: 2 mm test pieces were prepared by vulcanization on a flat vulcanizer. The tensile strength, elongation at break, 300% tensile stress, and tear strength of the materials were tested using a LLOYD electronic tensile testing machine in accordance with GB / T528-1998. The test temperature was (23 ± 2) °C and the tensile speed was 500 mm / min. The Shore A hardness of the materials was tested using an XY21 rubber hardness tester (Shanghai Chemical Machinery Plant No. 4) in accordance with GB / T531-1999.

[0086] (2) Flame retardant properties: The horizontal and vertical burning properties of the vulcanized rubber were tested using a CZF horizontal and vertical burning tester (produced by Nanjing Jiangning District Analytical Instrument Factory) in accordance with GB / T2408-1996. The oxygen index of the material was tested using a positive-3 oxygen index meter (produced by Nanjing Jiangning County Analytical Instrument Factory) in accordance with GB / T2406-1993.

[0087] Table 1

[0088]

[0089] By comparing the data of Examples 1-3 and Comparative Examples 1-2 in Table 1, it can be seen that the present invention uses aminosilane and polyborosiloxane to treat micron-sized magnesium hydroxide, so that the tensile strength and extrusion processing performance of the composite material are improved. At the same time, the grafted siloxane can migrate to the surface when the polymer system burns to form a ceramic carbon layer to protect the matrix and enhance the flame retardant effect. Secondly, the reinforcing effect of carbon black is better than that of nano-magnesium hydroxide. Adding stearic acid-modified nano-magnesium hydroxide will cause the strength of the material to decrease. This is because stearic acid-modified nano-magnesium hydroxide may improve its dispersion, but weaken the filler-rubber interface effect. Therefore, the double-bond silane coupling agent is used to treat carbon black to increase the interface bonding strength between the carbon black surface and the matrix, which further improves the mechanical properties of the material by improving the polymer filled with fillers, the dispersibility of the filler and the filler-polymer interface effect.

[0090] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

[0091] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

Claims

1. A method for preparing a flame retardant EPDM halogen-free elastic rubber material, characterized in that: The method comprises the following preparation steps: (1) Take the raw materials by weight; (2) Plasticize the EPDM rubber for 5-8 times, and then add zinc oxide, sodium stearate, accelerator EG-3, flame retardant system, homemade carbon black, plasticizer, sulfur and carbonizing agent in order for mixing; (3) Pass the mixed rubber through 6-10 times and make sheets; (4) The film is placed in a mold and heated and pressurized for vulcanization to obtain a flame-retardant EPDM halogen-free elastic rubber material.

2. The method for preparing a flame retardant EPDM halogen-free elastic rubber material according to claim 1, characterized in that: The weight parts of the raw materials in step (1) are:

3. The method for preparing a flame retardant EPDM halogen-free elastic rubber material according to claim 1, characterized in that: The flame retardant system in step (2) is modified micron-sized magnesium hydroxide powder.

4. The method for preparing a flame retardant EPDM halogen-free elastic rubber material according to claim 3, characterized in that: The preparation method of the modified micron-sized magnesium hydroxide powder comprises the following steps: mixing magnesium hydroxide powder and water at a mass ratio of 1:10-1:20 to prepare a slurry with a mass fraction of 5-7%, then heating the mixture to 40-45° C. and mixing the mixture in a constant temperature water bath, adjusting the stirring speed to 600-800 r / min, dropwise adding aminosilane in an amount of 0.1-0.2 times the mass of the magnesium hydroxide powder and polyborosiloxane in an amount of 0.2-0.3 times the mass of the magnesium hydroxide powder, mixing the mixture for 1-2 hours, filtering and washing the mixture, and finally drying the mixture in a vacuum drying oven at 60-65° C., followed by grinding the mixture to obtain the modified micron-sized magnesium hydroxide powder.

5. The method for preparing a flame retardant EPDM halogen-free elastic rubber material according to claim 1, characterized in that: The preparation method of the homemade carbon black in step (2) is: Mix carbon black and water in a mass ratio of 1:10-1:20, then heat to 60-75°C and mix in a constant temperature water bath, adjust the stirring speed to 600-800r / min, add 0.2-0.3 times the mass of carbon black double bond silane coupling agent dropwise, mix for 1-2h, filter and wash, and finally dry in a vacuum drying oven at 60-65°C, followed by grinding to obtain homemade carbon black.

6. The method for preparing a flame retardant EPDM halogen-free elastic rubber material according to claim 1, characterized in that: The carbon-forming agent in step (2) is prepared by mixing silicone rubber, borate, zinc stannate and organic clay in a mass ratio of 1:2:1:

3.

7. The method for preparing a flame retardant EPDM halogen-free elastic rubber material according to claim 1, characterized in that: The plasticizer in step (2) is prepared by mixing paraffin oil and dioctyl phthalate in a mass ratio of 2:

5.

8. The method for preparing a flame retardant EPDM halogen-free elastic rubber material according to claim 1, characterized in that: The vulcanization conditions in step (4) are 22-26 MPa, 170-175° C., and 10-15 min.