PS (polystyrene) wood-like foamed sheet with texture and preparation method of PS wood-like foamed sheet
The single-phase continuous island structure is formed by using polystyrene, glue powder and hard asphalt in PS imitation wood foamed plates, and the waste glue powder and modified nanomullite and modified slope strands are modified by microwave radiation. The problem of insufficient impact resistance of PS foamed sheets in the prior art has been solved, and good impact resistance and flame retardant properties have been achieved.
Patent Information
- Application Number
- CN202411209704.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
AI Technical Summary
The existing PS foamed sheets have poor flexibility due to the rigidity of the benzene ring, and the magnesium hydroxide flame retardant has an adverse effect on the mechanical properties, making it difficult to have good impact resistance and is not suitable for imitation with certain impact resistance requirements. Wood material.
Polystyrene, rubber powder and hard asphalt are used as base materials, combined with ethylene propylene rubber powder and PETG resin to form a single-phase continuous island structure. The hard asphalt is evenly dispersed in the form of super micelles, and ethylene propylene rubber powder absorbs impact and enhance impact resistance through microwave radiation modification of waste rubber powder, modified nanomullite and modified acetaminite.
It significantly improves the impact resistance and flame retardant properties of PS imitation wood foamed sheets, making them suitable for occasions with certain impact resistance requirements.
Smart Images

Figure BDA0005020021290000051 
Figure BDA0005020021290000061 
Figure BDA0005020021290000062
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of wood-like panels, and more specifically, to a PS wood-like foamed panel with a self-textured texture and a preparation method thereof. Background Art
[0002] Wood-like materials are a new type of materials that imitate the structure and properties of natural wood. In recent years, due to the shortage of wood resources and the increasing attention to environmental protection, the research and development of wood-like materials has received widespread attention. PS wood-like materials are an important type of wood-like materials, usually made of polystyrene as the base material and obtained after foaming. Since polystyrene has the characteristics of high transparency, high hardness, strong rigidity, heat resistance, corrosion resistance, easy dyeing, low moisture absorption, low price, and easy processing, PS wood-like materials are widely used in various fields of production and life.
[0003] In the related art, there is a PS foam board, which includes the following raw materials in parts by weight: 65 parts of base material, 5 parts of filler, 25 parts of magnesium hydroxide flame retardant, 0.1 parts of AC foaming agent, 0.3 parts of antioxidant, 0.5 parts of lubricant, and 0.5 parts of color powder. The base material is polystyrene and the filler is light calcium powder.
[0004] With respect to the above-mentioned related technologies, the inventors believe that in PS foam materials, the rigidity of the benzene ring will lead to poor flexibility of polystyrene, and the magnesium hydroxide flame retardant has an adverse effect on the mechanical properties, making it difficult for the PS foam board in the related technology to have good impact resistance and is not suitable for the production of imitation wood materials with certain impact resistance requirements. Summary of the invention
[0005] The PS foamed board in the related art is difficult to have good impact resistance and is not suitable for producing wood-like materials with certain impact resistance requirements. In order to improve this defect, the present application provides a PS wood-like foamed board with a self-textured texture and a preparation method thereof.
[0006] In the first aspect, the present application provides a PS imitation wood foam board with a self-texture, adopting the following technical scheme: a PS imitation wood foam board with a self-texture, comprising the following raw materials in parts by weight: 80-140 parts of a base material, 5-20 parts of a PETG resin, 5-10 parts of a filler, 25-35 parts of a magnesium hydroxide flame retardant, 0.1-1.5 parts of an AC foaming agent, 0.3-0.8 parts of an antioxidant, 0.5-2 parts of a lubricant, and 0.5-2 parts of a color powder; the components of the base material include polystyrene, rubber powder and hard asphalt, and the rubber powder includes ethylene propylene diene monomer rubber powder.
[0007] By adopting the above technical scheme, the present application preferably uses polystyrene, rubber powder and hard asphalt as base materials, and also limits the rubber powder to include EPDM rubber powder. In the wood-like foam board of the present application, EPDM rubber powder and PETG resin as dispersed phases in polystyrene have poor compatibility with polystyrene, forming a single-phase continuous island structure, which can present a pattern similar to the texture of natural wood on a macro scale. Hard asphalt has good compatibility with polystyrene and can be evenly dispersed in polystyrene in the form of super micelles. The hard asphalt super micelles dispersed in polystyrene can produce an "anchor effect", and EPDM rubber powder can absorb part of the impact energy. In addition, the acidic groups in the hard asphalt have an adhesion effect on the magnesium hydroxide flame retardant, thereby overcoming the defects in the relevant technology, so that the PS wood-like foam board with the addition of magnesium hydroxide flame retardant has good impact resistance and is suitable for occasions with certain impact resistance requirements.
[0008] Preferably, the amount of the rubber powder is 15-35% of the total weight of the base material.
[0009] By adopting the above technical solution, the present application optimizes the dosage range of the rubber powder. Within the above range, the PS imitation wood foam board has good impact resistance.
[0010] Preferably, the amount of the rubber powder is 25-35% of the total weight of the base material.
[0011] By adopting the above technical solution, the present application further optimizes the dosage range of the rubber powder, which helps to fully improve the impact resistance of the PS imitation wood foam board.
[0012] Preferably, the amount of the hard asphalt is 3-5% of the total weight of the base material.
[0013] By adopting the above technical scheme, on the basis of optimizing the amount of rubber powder, the present application further optimizes the amount of hard asphalt, which helps to fully improve the impact resistance of the PS imitation wood foam board.
[0014] Preferably, the rubber powder further comprises modified waste rubber powder, and the modified waste rubber powder is prepared according to the following method: A mixture of isopropanol and benzene is used as a solvent, the waste rubber powder is extracted until the solvent becomes colorless and then taken out, the extracted waste rubber powder is dried, and then subjected to microwave radiation treatment, and the irradiated waste rubber powder is immersed in styrene overnight to obtain modified waste rubber powder.
[0015] By adopting the above technical solution, the present application uses microwave radiation to modify the waste rubber powder. Microwave radiation can break some cross-linking bonds in the waste rubber powder molecules and increase the number of oxygen-containing groups on the surface of the waste rubber powder. Therefore, the bonding force between the surface of the modified waste rubber powder and polystyrene can be improved, which helps to enhance the impact resistance of the PS imitation wood foam board.
[0016] Preferably, the amount of the modified waste rubber powder is 4-8% of the total weight of the base material.
[0017] By adopting the above technical solution, the present application optimizes the proportion of modified waste rubber powder, which helps to fully improve the impact resistance of the PS imitation wood foam board.
[0018] Preferably, the filler comprises modified nano-mullite, and the modified nano-mullite is prepared according to the following method: adding nano-mullite to isopropanol and stirring and mixing, adding a mixture of a titanate coupling agent and isopropanol after ultrasonic dispersion, continuing ultrasonic dispersion for a period of time to obtain an emulsion, filtering the emulsion, and obtaining the modified nano-mullite after drying and grinding the filter cake.
[0019] By adopting the above technical solution, the present application uses titanate coupling agent to modify nano mullite, and obtains modified nano mullite with good compatibility with polystyrene. The modified nano mullite itself has good mechanical strength, and can play a toughening role on PS imitation wood foam board. By coordinating with polystyrene, rubber powder, hard asphalt, PETG resin, etc., the impact resistance of PS imitation wood foam board can be improved.
[0020] Preferably, the filler further comprises modified palygorskite, and the modified palygorskite is prepared according to the following method: The palygorskite and hydrochloric acid are mixed and heated in a water bath, and stirred while heating to obtain a mixture, the mixture is ultrasonically dispersed, and then the mixture is filtered to obtain a filter cake, the filter cake is washed and dried, and the modified palygorskite is obtained after grinding.
[0021] By adopting the above technical solution, the present application uses hydrochloric acid to modify palygorskite to obtain modified palygorskite. The modified palygorskite can improve the mechanical properties of polystyrene, and can also release crystal water during combustion, and has a synergistic flame retardant effect with magnesium hydroxide, which helps to improve the flame retardant properties of PS imitation wood foam board.
[0022] Preferably, the weight ratio of the modified nano-mullite to the modified palygorskite is 1:(1-2).
[0023] By adopting the above technical solution, the present application optimizes the weight ratio of modified nano-mullite and modified palygorskite, which helps to obtain a PS imitation wood foam board with good impact resistance and flame retardancy.
[0024] In a second aspect, the present application provides a method for preparing a PS imitation wood foam board with a self-textured texture, using the following technical solution.
[0025] A method for preparing a PS imitation wood foamed board with a self-textured texture comprises the following steps: (1) polystyrene and PETG resin are dried for standby use; (2) polystyrene, rubber powder and hard asphalt are mixed to obtain a base material, the base material and PETG resin are added to a mixer and mixed, and then fillers, magnesium hydroxide flame retardant, AC foaming agent, antioxidant, lubricant and toner are added to the mixer in sequence to obtain a rough mixture after stirring and mixing; (3) The crude mixture is melt-extruded and granulated at 160-200° C. to obtain foamed particles, and the board is extruded at 150-205° C. to obtain a PS imitation wood foam board with a self-textured texture.
[0026] By adopting the above technical solution, the present application first prepares the base material, then mixes the base material with other components, and then goes through two processes of extrusion granulation and board extrusion to obtain a PS imitation wood foam board with its own texture.
[0027] In summary, this application has the following beneficial effects: 1. This application preferably uses polystyrene, rubber powder and hard asphalt as base materials, and also specifies that the rubber powder includes EPDM rubber powder. Through the synergistic effect of hard asphalt, EPDM rubber powder and other components, the defects in the relevant technology are overcome, so that the PS imitation wood foam board with magnesium hydroxide flame retardant added has good impact resistance.
[0028] 2. The present application processes waste rubber powder by microwave radiation to obtain modified waste rubber powder. Microwave radiation can break some cross-linking bonds in the waste rubber powder molecules and increase the number of oxygen-containing groups on the surface of the waste rubber powder. Therefore, the bonding force between the surface of the modified waste rubber powder and polystyrene can be improved, which helps to enhance the impact resistance of the PS imitation wood foam board.
[0029] 3. The present application uses titanate coupling agent to modify nano-mullite, and obtains modified nano-mullite having good compatibility with polystyrene. The modified nano-mullite can improve the impact resistance of PS imitation wood foam board by synergistically coordinating with polystyrene, rubber powder, hard asphalt, PETG resin and equal parts.
[0030] 4. The present application uses hydrochloric acid to modify palygorskite to obtain modified palygorskite. The modified palygorskite can improve the mechanical properties of polystyrene, and can also release crystal water during combustion, and has a synergistic flame retardant effect with magnesium hydroxide, which helps to improve the flame retardant properties of PS imitation wood foam board. DETAILED DESCRIPTION
[0031] The present application is further described in detail below in conjunction with embodiments, preparation examples and comparative examples. The raw materials involved in the present application can all be obtained commercially.
[0032] Preparation example of modified waste rubber powder The following is an explanation using Preparation Example 1.
[0033] Preparation Example 1 In this preparation example, the waste rubber powder is 200-mesh styrene-butadiene rubber waste rubber powder.
[0034] In this preparation example, the modified waste rubber powder is prepared according to the following method: A mixture obtained by compounding isopropanol and benzene in a weight ratio of 1:1 is used as a solvent, the waste rubber powder is extracted until the solvent becomes colorless and then taken out, the extracted waste rubber powder is dried at 80°C, and then subjected to microwave radiation treatment for 300s under 200W conditions, and the irradiated waste rubber powder is immersed in styrene for 12h (i.e., soaked overnight) to obtain modified waste rubber powder.
[0035] Preparation example of modified nano-mullite The following is an explanation using Preparation Example 2.
[0036] Preparation Example 2 The nano-mullite used in this preparation example has an average length of 90 nm and an average diameter of 30 nm, and the titanate coupling agent is isopropyl dioleyloxy (dioctylphosphoacyloxy) titanate.
[0037] In this preparation example, the modified nano-mullite was prepared according to the following method: Nano-mullite was added to isopropanol at a weight ratio of 1:10 and stirred for 20 minutes. After ultrasonic dispersion for 20 minutes, a mixture prepared by a titanate coupling agent and isopropanol at a weight ratio of 1:3 was added at a volume ratio of 1:1. Ultrasonic dispersion was continued for 40 minutes to obtain an emulsion. The emulsion was filtered, and the filter cake was dried and ground to obtain modified nano-mullite.
[0038] Preparation example of modified palygorskite The following is an explanation using Preparation Example 3.
[0039] Preparation Example 3 In this preparation example, the modified palygorskite is prepared according to the following method:.
[0040] The palygorskite and 38wt% concentrated hydrochloric acid were mixed in a weight ratio of 1:10, and then 0.3mol / L dilute hydrochloric acid was added in a weight ratio of palygorskite:dilute hydrochloric acid=1:30, and the mixture was stirred for 120min in a 60°C water bath to obtain a mixture, the mixture was ultrasonically dispersed for 30min, and then the mixture was filtered to obtain a filter cake, the filter cake was washed with water and dried, and the modified palygorskite was obtained after grinding. Example
[0041] Examples 1-5 The following description is given by taking Example 1 as an example.
[0042] Example 1 This embodiment provides a PS imitation wood foam board with a self-textured texture, including the following raw materials: 80kg base material, 5kg PETG resin, 5kg filler, 25kg magnesium hydroxide flame retardant, 0.1kg AC foaming agent, 0.3kg antioxidant, 0.5kg lubricant, 0.5kg color powder; the base material is a mixture of polystyrene, rubber powder and hard asphalt, wherein the amount of rubber powder accounts for 15% of the total weight of the base material, the amount of hard asphalt accounts for 2% of the total weight of the base material, and the rest is polystyrene. The rubber powder is 200 mesh EPDM rubber powder, the softening point of hard asphalt is 141°C, and the model of polystyrene is PS-PG33. The melting point of PETG resin is 150°C, the filler is 325 mesh light calcium powder, the D50 particle size of magnesium hydroxide flame retardant is 0.5μm, the antioxidant is antioxidant 1010, and the lubricant is zinc stearate.
[0043] This embodiment provides a method for preparing a PS imitation wood foam board with a self-textured texture, comprising the following steps: (1) drying polystyrene and PETG resin at 85° C. for standby use; (2) polystyrene, rubber powder and hard asphalt are mixed to obtain a base material, the base material and PETG resin are added to a mixer and mixed, and then fillers, magnesium hydroxide flame retardant, AC foaming agent, antioxidant, lubricant and toner are added to the mixer in sequence to obtain a rough mixture after stirring and mixing; (3) The crude mixture is melt-extruded and granulated at 160° C. (referred to as T1, the same below) to obtain foamed particles, and then extruded into a board at 150° C. (referred to as T2, the same below) to obtain a PS imitation wood foam board with a self-textured texture.
[0044] As shown in Table 1, the differences between Examples 1-5 are mainly in the different raw material ratios and extrusion temperatures of the PS imitation wood foamed board.
[0045] Table 1 Raw material ratio and extrusion temperature Embodiment 5-9 As shown in Table 2, the difference between Examples 6-9 and Example 5 is that the percentage of the amount of rubber powder used in the total weight of the base material (referred to as the percentage of rubber powder) is different.
[0046] Table 2 Rubber powder ratio Examples 9-12 As shown in Table 3, the difference between Examples 10-12 and Example 9 is that the percentage of hard asphalt used in the total weight of the base material (referred to as hard asphalt ratio) is different.
[0047] Table 3 Hard asphalt ratio sample Hard asphalt ratio / % Example 9 2 Example 10 3 Embodiment 11 4 Example 12 5 Embodiment 13 The difference between this embodiment and embodiment 12 is that the rubber powder is mixed with EPDM rubber powder and the modified waste rubber powder of embodiment 1, and the amount of the modified waste rubber powder accounts for 2% of the total weight of the base material.
[0048] As shown in Table 4, the difference between Examples 13-16 is that the percentage of the amount of modified waste rubber powder in the total weight of the base material (referred to as the percentage of modified waste rubber powder) is different.
[0049] Table 4 Proportion of modified waste rubber powder sample Proportion of modified waste rubber powder / % Embodiment 13 2 Embodiment 14 4 Embodiment 15 6 Example 16 8 Embodiment 17 The difference between this embodiment and embodiment 16 is that the filler is formed by mixing light calcium powder and auxiliary filler in a weight ratio of 1:1, and the auxiliary filler is the modified nano-mullite of Preparation Example 2.
[0050] Embodiment 18 The difference between this embodiment and embodiment 17 is that the auxiliary filler is formed by mixing the modified nano-mullite of preparation example 2 and the modified palygorskite of preparation example 3 in a weight ratio of 1:1.
[0051] As shown in Table 5, the difference between Examples 18-20 is that the weight ratio of the modified nano-mullite and the modified palygorskite (hereinafter referred to as the auxiliary filler ratio) is different.
[0052] Table 5 Auxiliary filler ratio sample Auxiliary filler ratio Embodiment 18 1:1 Embodiment 19 1:1.5 Embodiment 20 1:2 Comparative Example Comparative Example 1 This comparative example provides a PS foamed board, including the following raw materials: 65kg of base material, 5kg of filler, 25kg of magnesium hydroxide flame retardant, 0.1kg of AC foaming agent, 0.3kg of antioxidant, 0.5kg of lubricant, and 0.5kg of color powder; the base material is polystyrene, and the model of polystyrene is PS-PG33. The filler is 325-mesh light calcium powder, the D50 particle size of the magnesium hydroxide flame retardant is 0.5μm, the antioxidant is antioxidant 1010, and the lubricant is zinc stearate.
[0053] This comparative example provides a method for preparing a PS foamed plate, comprising the following steps: (1) adding a base material, a filler, a magnesium hydroxide flame retardant, an AC foaming agent, an antioxidant, a lubricant and a toner into a blender to obtain a rough mixture; (2) The crude mixture was melt-extruded and granulated at 160°C to obtain foamed particles, and then extruded at 150°C to obtain a PS foamed sheet.
[0054] Comparative Example 2 The difference between this comparative example and Example 1 is that the base material does not include rubber powder.
[0055] Comparative Example 3 This comparative example is different from Example 1 in that the base material does not include hard asphalt.
[0056] Performance testing methods 1. Mechanical properties Taking impact strength as a representative of mechanical properties, the test was carried out in accordance with "ISO 179.1 2010 Determination of impact properties of simply supported beams of plastics - Part 1: Non-instrumented impact test". Taking the impact strength of Comparative Example 1 as a benchmark, the ratio between the impact strength of each embodiment and comparative example and the impact strength of Comparative Example 1 was calculated, and the ratio was recorded as relative impact strength. The results are shown in Table 6.
[0057] 2. Flame retardant properties With reference to the provisions of the Test Method for Combustion Performance of Plastic Materials (UL-94), the PS imitation wood (flame retardant) foam materials of each embodiment and comparative example were tested to test the total afterflame time. Then, based on the total afterflame time of comparative example 1, the ratio between the total afterflame time of each embodiment and comparative example and the total afterflame time of comparative example 1 was calculated, and the ratio was recorded as the relative afterflame time. The results are shown in Table 6.
[0058] Table 6 Relative impact strength and relative afterflame time Combining Examples 1-5 and Comparative Example 1 and Table 6, it can be seen that the impact strengths measured in Examples 1-5 are all higher than those in Comparative Example 1, indicating that Examples 1-5 overcome the defects in the related art through the synergistic effect of components such as hard asphalt and EPDM rubber powder, so that the PS imitation wood foam board with the addition of magnesium hydroxide flame retardant has good impact resistance.
[0059] It can be seen from Example 1 and Comparative Examples 2-3 and Table 6 that when the rubber powder is not used in combination with hard asphalt, the impact resistance of the PS imitation wood foam board is limited.
[0060] Combining Examples 5-9 and Table 6, it can be seen that when the amount of the rubber powder accounts for 15-35% of the total weight of the base material, the PS imitation wood foam board has good impact resistance. Among them, when the amount of the rubber powder accounts for 25-35% of the total weight of the base material, the impact resistance of the PS imitation wood foam board is better.
[0061] It can be seen from Example 9, Examples 10-12 and Table 6 that when the amount of hard asphalt accounts for 3-5% of the total weight of the base material, the impact resistance of the PS imitation wood foamed board is better.
[0062] Combining Example 12, Examples 13-16 and Table 6, it can be seen that the addition of modified waste rubber powder helps to improve the impact resistance of the PS imitation wood foam board, and when the amount of modified waste rubber powder accounts for 4-8% of the total weight of the base material, the impact resistance of the PS imitation wood foam board is better.
[0063] It can be seen from Example 16, Example 17 and Table 6 that when the filler includes modified nano-mullite, the impact resistance of the PS imitation wood foam board is better.
[0064] It can be seen from Example 17, Examples 18-20 and Table 6 that when the filler includes modified nano-mullite and modified palygorskite at the same time, and the weight ratio of modified nano-mullite to modified palygorskite is 1:(1-2), the impact resistance of the PS imitation wood foam board is better, and the afterflame time is shortened, indicating that the flame retardant performance is improved.
[0065] The above embodiments are merely explanations of the present application and are not limitations of the present application. After reading this specification, those skilled in the art may make modifications to the embodiments of the present application without any creative contribution as needed. However, as long as they are within the scope of the claims of the present application, they are protected by the patent law.
Claims
1. A PS imitation wood foam board with self-textured texture, characterized in that: The invention comprises the following raw materials in parts by weight: 80-140 parts of base material, 5-20 parts of PETG resin, 5-10 parts of filler, 25-35 parts of magnesium hydroxide flame retardant, 0.1-1.5 parts of AC foaming agent, 0.3-0.8 parts of antioxidant, 0.5-2 parts of lubricant and 0.5-2 parts of color powder; the components of the base material include polystyrene, rubber powder and hard asphalt, and the rubber powder includes EPDM rubber powder.
2. The PS imitation wood foam board with self-texture according to claim 1, characterized in that: The amount of the rubber powder is 15-35% of the total weight of the base material.
3. The PS imitation wood foam board with self-texture according to claim 2, characterized in that: The amount of the rubber powder is 25-35% of the total weight of the base material.
4. The PS imitation wood foam board with self-texture according to claim 3, characterized in that: The amount of the hard asphalt is 3-5% of the total weight of the base material.
5. The PS imitation wood foam board with self-texture according to claim 2, characterized in that: The rubber powder also includes modified waste rubber powder, and the modified waste rubber powder is prepared according to the following method: A mixture of isopropanol and benzene is used as a solvent, the waste rubber powder is extracted until the solvent becomes colorless and then taken out, the extracted waste rubber powder is dried, and then subjected to microwave radiation treatment, and the irradiated waste rubber powder is immersed in styrene overnight to obtain modified waste rubber powder.
6. The PS imitation wood foam board with self-texture according to claim 5, characterized in that: The amount of the modified waste rubber powder is 4-8% of the total weight of the base material.
7. The PS imitation wood foam board with self-texture according to claim 1, characterized in that: The filler includes modified nano-mullite, and the modified nano-mullite is prepared according to the following method: The nano-mullite is added into isopropanol and stirred and mixed. After ultrasonic dispersion, a mixture of titanate coupling agent and isopropanol is added. After ultrasonic dispersion for a period of time, an emulsion is obtained. The emulsion is filtered and the filter cake is dried and ground to obtain the modified nano-mullite.
8. The PS imitation wood foam board with self-texture according to claim 7, characterized in that: The filler further comprises modified palygorskite, and the modified palygorskite is prepared according to the following method: The palygorskite and hydrochloric acid are mixed and heated in a water bath, and stirred while heating to obtain a mixture, the mixture is ultrasonically dispersed, and then the mixture is filtered to obtain a filter cake, the filter cake is washed and dried, and the modified palygorskite is obtained after grinding.
9. The PS imitation wood foam board with self-texture according to claim 8, characterized in that: The weight ratio of the modified nano-mullite to the modified palygorskite is 1:(1-2).
10. The method for preparing the PS imitation wood foamed board with self-texture according to any one of claims 1 to 9, characterized in that: The following steps are involved: (1) Dry the polystyrene and PETG resins for later use; (2) polystyrene, rubber powder and hard asphalt are mixed to obtain a base material, the base material and PETG resin are added into a mixer and mixed, and then filler, magnesium hydroxide flame retardant, AC foaming agent, antioxidant, lubricant and color powder are added into the mixer in sequence, and a rough mixture is obtained after stirring and mixing; (3) The crude mixture is melt-extruded and granulated at 160-200° C. to obtain foamed particles, and the sheet is extruded at 150-205° C. to obtain a PS imitation wood foam sheet with a self-textured texture.