Medical micron-sized PTFE (Polytetrafluoroethylene) film with high mechanical property and preparation method of medical micron-sized PTFE film

Through the combination of polytetrafluoroethylene dispersion and acrylic emulsion, combined with specific process steps and parameter control, the problems of low preparation efficiency and uneven performance of polytetrafluoroethylene films in the prior art are solved, and the micrometer-level high Preparation of mechanical properties films to meet the needs of medical catheters.

CN119081319APending Publication Date: 2024-12-06M-DUKE MEDICAL TECH (SHANGHAI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311747211.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-12-19
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing polytetrafluoroethylene film preparation process is complex, has low efficiency, and it is difficult to obtain micron-level high mechanical properties films that meet medical catheters.

Method used

Using a combination of polytetrafluoroethylene dispersion and acrylic emulsion, micrometer-level high mechanical properties PTFE films are prepared by stirring, dipping, drying, sintering and cooling steps, controlling the average particle size and molecular weight distribution of polytetrafluoroethylene, combined with Specific sintering temperature and dip coating speed ensure uniform film thickness and performance.

Benefits of technology

The preparation process of polytetrafluoroethylene film is simplified, the elastic modulus and strength of the film is improved, the thickness requirements of medical catheters are met, and the performance uniformity and stability of the film is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004614726500000091
    Figure BDA0004614726500000091
Patent Text Reader

Abstract

The invention relates to the technical field of polytetrafluoroethylene film materials, in particular to the field of IPC B29K 27, and more particularly relates to a medical micron-sized high-mechanical-property PTFE film and a preparation method thereof. The preparation method comprises the following steps: S1, pretreatment: stirring a polytetrafluoroethylene dispersion liquid and an acrylic resin emulsion to uniformly disperse the polytetrafluoroethylene dispersion liquid and the acrylic resin emulsion to obtain a mixed solution; s2, dip-coating and drying: selecting a substrate, soaking the substrate in the mixed solution, standing, lifting, and drying after the substrate uniformly flows in the gravity direction; s3, sintering: carrying out sintering treatment on the polytetrafluoroethylene layer after dip-coating; and S4, cooling: after the sintered material is cooled to room temperature, stripping the polytetrafluoroethylene from the substrate to obtain the composite material. Through the specific dip-coating process and the sintering temperature for controlling the crystallinity, the prepared thin film is simplified in process and has high elastic modulus and tensile strength at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polytetrafluoroethylene film materials, in particular to the field of IPC B29K 27, and more specifically to a medical micron-level high-mechanical-performance PTFE film and a preparation method thereof. Background Art

[0002] Polytetrafluoroethylene (PTFE) film materials have strong high and low temperature resistance, hydrophobicity, non-stickiness, self-lubrication, corrosion resistance and friction resistance, and are widely used in clothing, medical, electronics and other fields. In recent years, especially in the field of medical catheters, polytetrafluoroethylene film catheters are often used as the innermost layer of the catheter and combined with other materials. The polytetrafluoroethylene film in the prior art is made of polytetrafluoroethylene powder as the main raw material and is prepared by molding, extrusion and other processes.

[0003] CN 111016206 B discloses a method for preparing a polytetrafluoroethylene film with good bending fatigue resistance, comprising the steps of: sieving polytetrafluoroethylene suspension resin powder through a 10-mesh screen, and then obtaining a turning film by molding, sintering, and turning; heat-stretching the turning film under the condition of being greater than or equal to the glass transition temperature of the polytetrafluoroethylene resin and less than the melting temperature of the polytetrafluoroethylene resin; after heat-stretching, lowering the temperature to below the glass transition temperature to obtain a polytetrafluoroethylene film. The preparation process is suitable for mass production of polytetrafluoroethylene products. However, the process flow is long and complicated, and the efficiency is low for the production of polytetrafluoroethylene pipes of thin films, and the film thickness is high, and it cannot meet the use in the field of medical catheters. Summary of the invention

[0004] The first aspect of the present invention provides a medical micron-level PTFE film with high mechanical properties, the raw materials of which include: polytetrafluoroethylene dispersion and acrylic resin emulsion.

[0005] Preferably, the solid content of the polytetrafluoroethylene dispersion is 30-60%, and the viscosity (25°C) is (16-30) x 10 -3 Pa·s.

[0006] The average particle size of polytetrafluoroethylene in the polytetrafluoroethylene dispersion is 0.15-0.40 μm, and the molecular weight distribution of polytetrafluoroethylene is 1.3-2.2.

[0007] Further preferably, the polytetrafluoroethylene dispersion is purchased from Daikin Industries, Ltd., model: D-110.

[0008] The acrylic resin emulsion includes at least one of methyl acrylate emulsion, ethyl acrylate emulsion, methyl methacrylate emulsion, ethyl methacrylate emulsion and copolymerized acrylic acid monomer emulsion.

[0009] Preferably, the copolymerized acrylic monomer emulsion contains at least two of vinyl acetate, styrene, acrylonitrile, dibutyl maleate and butadiene.

[0010] The acrylic resin emulsion has a solid content of 35-50% and a viscosity (25° C.) of 2-40 mPa·s.

[0011] Preferably, the acrylic resin emulsion has a solid content of 39-41% and a viscosity (25° C.) of 2-40 mPa·s.

[0012] Further preferably, the acrylic resin emulsion is purchased from Showa Polymer Co., Ltd., model: methyl acrylate.

[0013] The applicant has found that the solid content of the polytetrafluoroethylene dispersion is 30-60%, and the viscosity (25°C) is (16-30) x 10 -3 Pa·s and controlling the average particle size of polytetrafluoroethylene to 0.15-0.40μm, the molecular weight distribution of polytetrafluoroethylene to 1.3-2.2, can effectively improve the film-forming performance of the mixed solution, so that it can be used for dipping process, while the PTFE emulsion concentration is too low, the film-forming property is poor; the concentration is too high, the film-forming is uneven. At the same time, with a specific solid content of 35-50%, the viscosity (25°C) of 2-40mPa·s acrylic emulsion, the system viscosity can be controlled, the film-forming performance can be further improved, and at the same time, it can be matched with a specific immersion and lifting speed, and the thickness of the polytetrafluoroethylene film can be effectively controlled to be 2-10μm, meeting the thickness requirements of medical catheters.

[0014] The weight ratio of the polytetrafluoroethylene dispersion to the acrylic resin emulsion is (10-20):1.

[0015] Preferably, the weight ratio of the polytetrafluoroethylene dispersion to the acrylic resin emulsion is 15:1, 10:1 or 12:1.

[0016] The second aspect of the present invention provides a method for preparing a medical micron-grade PTFE film with high mechanical properties, comprising the following steps:

[0017] S1. Pretreatment: stirring the polytetrafluoroethylene dispersion and the acrylic resin emulsion to make them dispersed evenly to obtain a mixed solution;

[0018] S2, dipping and drying: select a substrate, immerse it in the mixed solution, let it stand, then lift it up, wait for it to flow evenly in the direction of gravity, and then dry it;

[0019] S3, sintering: the dip-coated polytetrafluoroethylene layer is sintered;

[0020] S4, cooling: after the sintered material is cooled to room temperature, the polytetrafluoroethylene is peeled off from the substrate to obtain the product.

[0021] Preferably, the immersion speed is 2-10 mm / s, and the lifting speed is 2-30 mm / s.

[0022] Preferably, the drying temperature is 100-140° C., and the drying time is 10-40 min.

[0023] The applicant has found that after the dip coating process, the specific sintering temperature is 340-360°C, which can effectively increase the film crystallinity to between 35-45%, thereby simultaneously improving the elastic modulus and strength, making it much higher than the existing products with a crystallinity of 20%-30%. It may be that the specific sintering temperature affects the movement of the polymer chains in the crystalline and amorphous regions. Further research has found that the standing time of 10-50s can effectively improve the uniformity of the film thickness. If the standing time is short, the contact between the emulsion and the substrate is insufficient, and the polytetrafluoroethylene particles are unevenly distributed on the substrate; if the standing time is long, the PTFE particles in the emulsion settle in the container and are also unevenly distributed on the substrate. The final manifestation is uneven film thickness.

[0024] Preferably, the standing time is 10-50s.

[0025] Preferably, the sintering temperature is 340-360°C.

[0026] Beneficial effects:

[0027] 1. The solid content of the polytetrafluoroethylene dispersion is 30-60%, and the viscosity (25°C) is (16-30) x 10 -3 Pa

[0028] ·s and controlling the average particle size of polytetrafluoroethylene to 0.15-0.40μm and the molecular weight distribution of polytetrafluoroethylene to 1.3-2.2 can effectively improve the film-forming performance of the mixed solution.

[0029] 2. The immersion speed is 2-10 mm / s, and the lifting speed is 2-30 mm / s, which can effectively control the thickness of the polytetrafluoroethylene film to be 2-10 μm, meeting the thickness requirements of medical catheters.

[0030] 3. The present application uses a specific dip-coating process, which is easy to operate and can simplify the process of preparing polytetrafluoroethylene film for application catheters. At the same time, the parameters are easy to control, thereby improving the performance uniformity and stability of the film.

[0031] 4. The sintering temperature is 340-360°C, so that the prepared film has high elastic modulus and tensile strength. DETAILED DESCRIPTION

[0032] Example 1

[0033] The invention discloses a medical micron-level PTFE film with high mechanical properties, the raw materials of which are polytetrafluoroethylene dispersion and acrylic resin emulsion.

[0034] The weight ratio of the polytetrafluoroethylene dispersion to the acrylic resin emulsion is 15:1.

[0035] The polytetrafluoroethylene dispersion was purchased from Daikin Industries, Ltd., model: D-110.

[0036] The acrylic resin emulsion was purchased from Showa Polymer Co., Ltd., model: methyl acrylate.

[0037] A method for preparing a medical micron-grade PTFE film with high mechanical properties comprises the following steps:

[0038] S1. Pretreatment: Stir the polytetrafluoroethylene dispersion and the acrylic resin emulsion on a magnetic stirrer for 1 hour to make them dispersed evenly to obtain a mixed solution;

[0039] S2, dipping and drying: select a glass substrate, immerse it in the mixed solution, let it stand, then lift it up, wait for it to flow evenly in the direction of gravity, and then dry it;

[0040] S3, sintering: the dip-coated polytetrafluoroethylene layer is sintered;

[0041] S4, cooling: after the sintered material is cooled to room temperature, the polytetrafluoroethylene is peeled off from the substrate to obtain the product.

[0042] The immersion speed is 3 mm / s, and the lifting speed is 1 mm / s.

[0043] The drying temperature is 120° C. and the drying time is 20 min.

[0044] The standing time is 20s.

[0045] The sintering temperature is 360°C.

[0046] Example 2

[0047] The invention discloses a medical micron-level PTFE film with high mechanical properties, the raw materials of which are polytetrafluoroethylene dispersion and acrylic resin emulsion.

[0048] The weight ratio of the polytetrafluoroethylene dispersion to the acrylic resin emulsion is 15:1.

[0049] The polytetrafluoroethylene dispersion was purchased from Daikin Industries, Ltd., model: D-110.

[0050] The acrylic resin emulsion was purchased from Showa Polymer Co., Ltd., model: methyl acrylate.

[0051] A method for preparing a medical micron-grade PTFE film with high mechanical properties comprises the following steps:

[0052] S1. Pretreatment: Stir the polytetrafluoroethylene dispersion and the acrylic resin emulsion on a magnetic stirrer for 1 hour to make them dispersed evenly to obtain a mixed solution;

[0053] S2, dipping and drying: select a glass substrate, immerse it in the mixed solution, let it stand, then lift it up, wait for it to flow evenly in the direction of gravity, and then dry it;

[0054] S3, sintering: the dip-coated polytetrafluoroethylene layer is sintered;

[0055] S4, cooling: after the sintered material is cooled to room temperature, the polytetrafluoroethylene is peeled off from the substrate to obtain the product.

[0056] The immersion speed is 3 mm / s, and the lifting speed is 2 mm / s.

[0057] The drying temperature is 120° C. and the drying time is 20 min.

[0058] The standing time is 20s.

[0059] The sintering temperature is 360°C.

[0060] Example 3

[0061] The invention discloses a medical micron-level PTFE film with high mechanical properties, the raw materials of which are polytetrafluoroethylene dispersion and acrylic resin emulsion.

[0062] The weight ratio of the polytetrafluoroethylene dispersion to the acrylic resin emulsion is 15:1.

[0063] The polytetrafluoroethylene dispersion was purchased from Daikin Industries, Ltd., model: D-110.

[0064] The acrylic resin emulsion was purchased from Showa Polymer Co., Ltd., model: methyl acrylate.

[0065] A method for preparing a medical micron-grade PTFE film with high mechanical properties comprises the following steps:

[0066] S1. Pretreatment: Stir the polytetrafluoroethylene dispersion and the acrylic resin emulsion on a magnetic stirrer for 1 hour to make them dispersed evenly to obtain a mixed solution;

[0067] S2, dipping and drying: select a glass substrate, immerse it in the mixed solution, let it stand, then lift it up, wait for it to flow evenly in the direction of gravity, and then dry it;

[0068] S3, sintering: the dip-coated polytetrafluoroethylene layer is sintered;

[0069] S4, cooling: after the sintered material is cooled to room temperature, the polytetrafluoroethylene is peeled off from the substrate to obtain the product.

[0070] The immersion speed is 3 mm / s, and the lifting speed is 4 mm / s.

[0071] The drying temperature is 120° C. and the drying time is 20 min.

[0072] The standing time is 20s.

[0073] The sintering temperature is 360°C.

[0074] Example 4

[0075] The invention discloses a medical micron-level PTFE film with high mechanical properties, the raw materials of which are polytetrafluoroethylene dispersion and acrylic resin emulsion.

[0076] The weight ratio of the polytetrafluoroethylene dispersion to the acrylic resin emulsion is 15:1.

[0077] The polytetrafluoroethylene dispersion was purchased from Daikin Industries, Ltd., model: D-110.

[0078] The acrylic resin emulsion was purchased from Showa Polymer Co., Ltd., model: methyl acrylate.

[0079] A method for preparing a medical micron-grade PTFE film with high mechanical properties comprises the following steps:

[0080] S1. Pretreatment: Stir the polytetrafluoroethylene dispersion and the acrylic resin emulsion on a magnetic stirrer for 1 hour to make them dispersed evenly to obtain a mixed solution;

[0081] S2, dipping and drying: select a glass substrate, immerse it in the mixed solution, let it stand, then lift it up, wait for it to flow evenly in the direction of gravity, and then dry it;

[0082] S3, sintering: the dip-coated polytetrafluoroethylene layer is sintered;

[0083] S4, cooling: after the sintered material is cooled to room temperature, the polytetrafluoroethylene is peeled off from the substrate to obtain the product.

[0084] The immersion speed is 3 mm / s, and the lifting speed is 7 mm / s.

[0085] The drying temperature is 120° C. and the drying time is 20 min.

[0086] The standing time is 20s.

[0087] The sintering temperature is 360°C.

[0088] Example 5

[0089] The invention discloses a medical micron-level PTFE film with high mechanical properties, the raw materials of which are polytetrafluoroethylene dispersion and acrylic resin emulsion.

[0090] The weight ratio of the polytetrafluoroethylene dispersion to the acrylic resin emulsion is 15:1.

[0091] The polytetrafluoroethylene dispersion was purchased from Daikin Industries, Ltd., model: D-110.

[0092] The acrylic resin emulsion was purchased from Showa Polymer Co., Ltd., model: methyl acrylate.

[0093] A method for preparing a medical micron-grade PTFE film with high mechanical properties comprises the following steps:

[0094] S1. Pretreatment: Stir the polytetrafluoroethylene dispersion and the acrylic resin emulsion on a magnetic stirrer for 1 hour to make them dispersed evenly to obtain a mixed solution;

[0095] S2, dipping and drying: select a glass substrate, immerse it in the mixed solution, let it stand, then lift it up, wait for it to flow evenly in the direction of gravity, and then dry it;

[0096] S3, sintering: the dip-coated polytetrafluoroethylene layer is sintered;

[0097] S4, cooling: after the sintered material is cooled to room temperature, the polytetrafluoroethylene is peeled off from the substrate to obtain the product.

[0098] The immersion speed is 3 mm / s, and the lifting speed is 9 mm / s.

[0099] The drying temperature is 120° C. and the drying time is 20 min.

[0100] The standing time is 20s.

[0101] The sintering temperature is 360°C.

[0102] Example 6

[0103] The invention discloses a medical micron-level PTFE film with high mechanical properties, the raw materials of which are polytetrafluoroethylene dispersion and acrylic resin emulsion.

[0104] The weight ratio of the polytetrafluoroethylene dispersion to the acrylic resin emulsion is 15:1.

[0105] The polytetrafluoroethylene dispersion was purchased from Daikin Industries, Ltd., model: D-110.

[0106] The acrylic resin emulsion was purchased from Showa Polymer Co., Ltd., model: methyl acrylate.

[0107] A method for preparing a medical micron-grade PTFE film with high mechanical properties comprises the following steps:

[0108] S1. Pretreatment: Stir the polytetrafluoroethylene dispersion and the acrylic resin emulsion on a magnetic stirrer for 1 hour to make them dispersed evenly to obtain a mixed solution;

[0109] S2, dipping and drying: select a glass substrate, immerse it in the mixed solution, let it stand, then lift it up, wait for it to flow evenly in the direction of gravity, and then dry it;

[0110] S3, sintering: the dip-coated polytetrafluoroethylene layer is sintered;

[0111] S4, cooling: after the sintered material is cooled to room temperature, the polytetrafluoroethylene is peeled off from the substrate to obtain the product.

[0112] The immersion speed is 3 mm / s, and the lifting speed is 15 mm / s.

[0113] The drying temperature is 120° C. and the drying time is 20 min.

[0114] The standing time is 20s.

[0115] The sintering temperature is 360°C.

[0116] Example 7

[0117] The invention discloses a medical micron-level PTFE film with high mechanical properties, the raw materials of which are polytetrafluoroethylene dispersion and acrylic resin emulsion.

[0118] The weight ratio of the polytetrafluoroethylene dispersion to the acrylic resin emulsion is 15:1.

[0119] The polytetrafluoroethylene dispersion was purchased from Daikin Industries, Ltd., model: D-110.

[0120] The acrylic resin emulsion was purchased from Showa Polymer Co., Ltd., model: methyl acrylate.

[0121] A method for preparing a medical micron-grade PTFE film with high mechanical properties comprises the following steps:

[0122] S1. Pretreatment: Stir the polytetrafluoroethylene dispersion and the acrylic resin emulsion on a magnetic stirrer for 1 hour to make them dispersed evenly to obtain a mixed solution;

[0123] S2, dipping and drying: select a glass substrate, immerse it in the mixed solution, let it stand, then lift it up, wait for it to flow evenly in the direction of gravity, and then dry it;

[0124] S3, sintering: the dip-coated polytetrafluoroethylene layer is sintered;

[0125] S4, cooling: after the sintered material is cooled to room temperature, the polytetrafluoroethylene is peeled off from the substrate to obtain the product.

[0126] The immersion speed is 3 mm / s, and the lifting speed is 20 mm / s.

[0127] The drying temperature is 120° C. and the drying time is 20 min.

[0128] The standing time is 20s.

[0129] The sintering temperature is 360°C.

[0130] Example 8

[0131] The invention discloses a medical micron-level PTFE film with high mechanical properties, the raw materials of which are polytetrafluoroethylene dispersion and acrylic resin emulsion.

[0132] The weight ratio of the polytetrafluoroethylene dispersion to the acrylic resin emulsion is 15:1.

[0133] The polytetrafluoroethylene dispersion was purchased from Daikin Industries, Ltd., model: D-110.

[0134] The acrylic resin emulsion was purchased from Showa Polymer Co., Ltd., model: methyl acrylate.

[0135] A method for preparing a medical micron-grade PTFE film with high mechanical properties comprises the following steps:

[0136] S1. Pretreatment: Stir the polytetrafluoroethylene dispersion and the acrylic resin emulsion on a magnetic stirrer for 1 hour to make them dispersed evenly to obtain a mixed solution;

[0137] S2, dipping and drying: select a glass substrate, immerse it in the mixed solution, let it stand, then lift it up, wait for it to flow evenly in the direction of gravity, and then dry it;

[0138] S3, sintering: the dip-coated polytetrafluoroethylene layer is sintered;

[0139] S4, cooling: after the sintered material is cooled to room temperature, the polytetrafluoroethylene is peeled off from the substrate to obtain the product.

[0140] The immersion speed is 3 mm / s, and the lifting speed is 1 mm / s.

[0141] The drying temperature is 120° C. and the drying time is 20 min.

[0142] The standing time is 20s.

[0143] The sintering temperature is 340°C.

[0144] Example 9

[0145] The invention discloses a medical micron-level PTFE film with high mechanical properties, the raw materials of which are polytetrafluoroethylene dispersion and acrylic resin emulsion.

[0146] The weight ratio of the polytetrafluoroethylene dispersion to the acrylic resin emulsion is 15:1.

[0147] The polytetrafluoroethylene dispersion was purchased from Daikin Industries, Ltd., model: D-110.

[0148] The acrylic resin emulsion was purchased from Showa Polymer Co., Ltd., model: methyl acrylate.

[0149] A method for preparing a medical micron-grade PTFE film with high mechanical properties comprises the following steps:

[0150] S1. Pretreatment: Stir the polytetrafluoroethylene dispersion and the acrylic resin emulsion on a magnetic stirrer for 1 hour to make them dispersed evenly to obtain a mixed solution;

[0151] S2, dipping and drying: select a glass substrate, immerse it in the mixed solution, let it stand, then lift it up, wait for it to flow evenly in the direction of gravity, and then dry it;

[0152] S3, sintering: the dip-coated polytetrafluoroethylene layer is sintered;

[0153] S4, cooling: after the sintered material is cooled to room temperature, the polytetrafluoroethylene is peeled off from the substrate to obtain the product.

[0154] The immersion speed is 3 mm / s, and the lifting speed is 1 mm / s.

[0155] The drying temperature is 120° C. and the drying time is 20 min.

[0156] The standing time is 20s.

[0157] The sintering temperature is 350°C.

[0158] Comparative Example 1

[0159] Specific implementation method is the same as Example 1, except that the sintering temperature is 280°C.

[0160] Performance Testing Methods

[0161] The films in the embodiments and comparative examples were subjected to performance tests, and the test data are listed in Table 1.

[0162] 1) Crystallinity: The crystallinity is obtained by X-ray diffraction test and then analysis and calculation of the test results.

[0163] 2) Film thickness: measured by differential scanning calorimetry (DSC), calculating the heat absorbed during the melting process and comparing it with the heat absorption value of complete crystallization.

[0164] 3) Elastic modulus: Measured by a digital thickness gauge, where the thickness of each sample is tested at five points and the average value is taken.

[0165] 4) Stress at 25% strain: tensile test was performed using a dynamic thermomechanical analyzer.

[0166] Comparative Example 1 was unable to form a film and was not tested.

[0167] Performance test data

[0168] Table 1

[0169]

[0170] Combining Examples 1, 8, and 9 with Table 1, it can be seen that an increase in crystallinity will lead to an increase in the Young's modulus of the film. The elastic modulus of Examples 1, 8, and 9 is higher than 98.37 MPa, and the stress at 25% strain is higher than 6.939 MPa. In summary, by controlling different sintering conditions, the crystallinity of the finished film is different, and then different moduli are exhibited in the tensile test. The crystallinity increases from 38.4% to 43.35%, and the elastic modulus of the film increases by 23.4%.

Claims

1. A medical micron-grade PTFE film with high mechanical properties, characterized in that: Ingredients include: Polytetrafluoroethylene dispersion and acrylic resin emulsion.

2. A medical micron-grade high mechanical property PTFE film according to claim 1, characterized in that: The solid content of the polytetrafluoroethylene dispersion is 30-60%, and the viscosity is (16-30) x 10 -3 Pa·s.

3. A medical micron-grade high mechanical property PTFE film according to claim 2, characterized in that: The average particle size of polytetrafluoroethylene in the polytetrafluoroethylene dispersion is 0.15-0.40 μm, and the molecular weight distribution of polytetrafluoroethylene is 1.3-2.

2.

4. A medical micron-grade high mechanical property PTFE film according to claim 1 or 3, characterized in that: The acrylic resin emulsion includes at least one of methyl acrylate emulsion, ethyl acrylate emulsion, methyl methacrylate emulsion, ethyl methacrylate emulsion and copolymerized acrylic acid monomer emulsion.

5. A medical micron-grade high mechanical property PTFE film according to claim 4, characterized in that: The acrylic resin emulsion has a solid content of 35-50% and a viscosity of 2-40 mPa·s.

6. A medical micron-grade high mechanical property PTFE film according to claim 5, characterized in that: The weight ratio of the polytetrafluoroethylene dispersion to the acrylic resin emulsion is (10-20):

1.

7. A method for preparing a medical micron-grade PTFE film with high mechanical properties according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. Pretreatment: stirring the polytetrafluoroethylene dispersion and the acrylic resin emulsion to make them dispersed evenly to obtain a mixed solution; S2, dipping and drying: select a substrate, immerse it in the mixed solution, let it stand, then lift it up, wait for it to flow evenly in the direction of gravity, and then dry it; S3, sintering: the polytetrafluoroethylene layer after dip coating is sintered; S4, cooling: after the sintered material is cooled to room temperature, the polytetrafluoroethylene is peeled off from the substrate to obtain the product.

8. The method for preparing a medical micron-grade PTFE film with high mechanical properties according to claim 7, characterized in that: The immersion speed is 2-10 mm / s, and the lifting speed is 2-30 mm / s.

9. The method for preparing a medical micron-grade PTFE film with high mechanical properties according to claim 8, characterized in that: The standing time is 10-50s.

10. The method for preparing a medical micron-grade PTFE film with high mechanical properties according to claim 9, characterized in that: The sintering temperature is 340-360°C.