Wear-resistant and impact-resistant polymer floor and preparation process thereof

The polymer floor is enhanced with a cross-linked network and sacrificial bonds, addressing wear and impact resistance issues while providing self-repairing capabilities, thus reducing maintenance and enhancing safety.

CN119081323APending Publication Date: 2024-12-06GEMA NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411462658.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-19
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Traditional polymer flooring lacks wear resistance, impact resistance, and self-repairing capabilities, leading to increased maintenance costs and safety hazards in public spaces.

Method used

A wear-resistant and impact-resistant polymer floor is prepared by reacting pre-modified polyvinyl chloride with thiolated carbamoylphenylboronic acid and thiolated benzisothiazolinone, and pre-modified nano-silicon dioxide with 4-formylchlorophenylboronic acid, followed by kneading and calendering to introduce a cross-linked network and sacrificial bonds for enhanced mechanical properties.

Benefits of technology

The resulting polymer floor exhibits excellent wear resistance, impact resistance, and self-repairing capabilities at room temperature, reducing maintenance costs and improving safety.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a wear-resistant and impact-resistant polymer floor and a preparation process thereof, and relates to the technical field of floors. When the wear-resistant and impact-resistant polymer floor is prepared, polyvinyl chloride and sodium hydroxide react to prepare pre-modified polyvinyl chloride; the pre-modified polyvinyl chloride, sulfhydrylated carbamoyl phenylboronic acid and sulfhydrylated benzisothiazolinone are subjected to a reaction, and modified polyvinyl chloride is prepared; carrying out polymerization growth on bis (oxirane methyl) phenyl phosphate and 1, 5-diaminonaphthalene on the pretreated nano silicon dioxide to prepare pre-modified nano silicon dioxide; reacting the pre-modified nano silicon dioxide with 4-formyl chlorobenzene boric acid to obtain modified nano silicon dioxide; the modified polyvinyl chloride and the modified nano silicon dioxide are internally mixed and then subjected to calendaring molding, and the wear-resistant and impact-resistant polymer floor is prepared. The wear-resistant and impact-resistant polymer floor prepared by the invention has excellent flame-retardant, antibacterial, self-repairing, wear-resistant and impact-resistant properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of flooring, in particular to a wear-resistant and impact-resistant polymer flooring and a preparation process thereof. Background Art

[0002] Polymer flooring is a floor made of polymer materials. As a new type of flooring material that meets the requirements of energy conservation, emission reduction and sustainable development advocated by the country, polymer flooring has received close attention since its launch, and has aroused great interest from consumers and developers. From the perspective of environmental protection, traditional interior decoration materials are mainly composed of stone, wood, concrete and other materials, but first of all, most of them are not environmentally friendly. For example, composite flooring is made of high-quality hardwood, and the raw materials of natural marble are mineral resources with limited output. The mining and excavation of stone and the felling of wood are contrary to the sustainable development goal of harmony between man and nature; secondly, from the perspective of economy and maintenance convenience, compared with traditional flooring and other traditional flooring materials, polymer flooring has more advantages in price and maintenance. Wood flooring is not only expensive to buy, but also time-consuming and labor-intensive to maintain in the later stage. It needs to be cleaned and waxed regularly. If the laying area is large, it will take a lot of manpower, material resources and financial resources to clean and maintain it. The odor generated during the maintenance process such as waxing will also make people uncomfortable. The waxed floor sometimes feels greasy and slippery, which is easy to cause safety hazards when laid in public places. Polymer flooring is not only relatively affordable, but also eliminates the trouble of regular waxing and maintenance, and is easier to clean, greatly reducing the pressure of cleaning and maintenance during use, so it is very suitable for large public places.

[0003] Polymer floors are widely used in crowded places such as hospitals, kindergartens, nursing homes, playgrounds, laboratories, and factories. Polymer floors are required to have excellent wear resistance and impact resistance to extend their service life. Secondly, polymer floors prepared by traditional processes do not have self-repairing capabilities. After being scratched and punctured, their mechanical properties decrease, and the cost of repair and maintenance increases. In order to further improve the service life of polymer floors and reduce repair and maintenance costs, this application proposes a wear-resistant and impact-resistant polymer floor and its preparation process. The prepared polymer floor not only has excellent wear resistance and impact resistance, but can also self-repair at room temperature, which has important practical significance and broad market prospects. Summary of the invention

[0004] The purpose of the present invention is to provide a wear-resistant and impact-resistant polymer floor and a preparation process thereof, so as to solve the problems existing in the prior art.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: A wear-resistant and impact-resistant polymer floor, wherein the wear-resistant and impact-resistant polymer floor is prepared by reacting pre-modified polyvinyl chloride, thiolated carbamoylphenylboronic acid and thiolated benzisothiazolinone to obtain modified polyvinyl chloride; reacting pre-modified nano-silicon dioxide and 4-formylchlorophenylboronic acid to obtain modified nano-silicon dioxide; and kneading the modified polyvinyl chloride and the modified nano-silicon dioxide and then rolling them into a shape; The thiolated carbamoylphenylboronic acid is prepared by reacting 4-formylchlorophenylboronic acid and 3-mercapto-1-propylamine; The thiolated benzisothiazolinone is prepared by reacting 1,2-benzisothiazolin-3-one and 3-chloro-1-propanethiol; The pre-modified polyvinyl chloride is prepared by reacting polyvinyl chloride and sodium hydroxide; The pre-modified nano-silica is prepared by polymerizing bis(oxiranylmethyl)phenyl phosphate and 1,5-diaminonaphthalene on pre-treated nano-silica. The pretreated nano silicon dioxide is prepared by reacting nano silicon dioxide and 3-aminopropyltriethoxysilane.

[0006] A preparation process of a wear-resistant and impact-resistant polymer floor, the preparation process of the wear-resistant and impact-resistant polymer floor comprising the following preparation steps: (1) Add 4-formyl chlorophenylboronic acid and 3-mercapto-1-propylamine in a molar ratio of 1:1 to tetrahydrofuran (8 to 10 times the mass of 4-formyl chlorophenylboronic acid), add triethylamine (0.03 to 0.05 times the mass of 4-formyl chlorophenylboronic acid), stir at 10 to 30°C and 300 to 500 r / min for 2 to 3 hours, and dry at 50 to 60°C under vacuum for 7 to 8 hours to obtain thiolated carbamoylphenylboronic acid; Add 1,2-benzisothiazolin-3-one and 3-chloro-1-propanethiol in a molar ratio of 1:1 to tetrahydrofuran (8 to 10 times the mass of 1,2-benzisothiazolin-3-one), add triethylamine (0.03 to 0.05 times the mass of 1,2-benzisothiazolin-3-one), stir at 40 to 50°C and 300 to 500 r / min for 2 to 3 hours, and dry at 50 to 60°C under vacuum for 7 to 8 hours to obtain thiolated benzisothiazolinone; (2) Pre-modified polyvinyl chloride, thiolated carbamoylphenylboronic acid, thiolated benzisothiazolinone, azobisisobutyronitrile, and N,N-dimethylformamide are mixed uniformly in a mass ratio of 1:(0.3-0.4):(0.2-0.3):(0.03-0.05):(10-12), stirred at 70-80°C and 300-500 r / min for 3-4 hours, and dried at 50-60°C under vacuum conditions for 8-10 hours to obtain modified polyvinyl chloride; (3) Add bis(oxiranylmethyl)phenyl phosphate and 1,5-diaminonaphthalene in a molar ratio of 1:(1.2-1.3) to toluene with a mass of 12-14 times that of bis(oxiranylmethyl)phenyl phosphate, add pretreated nano-silica with a mass of 0.6-0.8 times that of bis(oxiranylmethyl)phenyl phosphate, stir at 50-60°C and 300-500 r / min for 4-6 hours, filter, wash with anhydrous ethanol 3-5 times, and vacuum at 50-60°C. Dry at 60°C for 8-10 hours to obtain pre-modified nano-silica; mix pre-modified nano-silica, 4-formylchlorophenylboronic acid, triethylamine and tetrahydrofuran in a mass ratio of 1:(2-3):(0.03-0.05):(10-12) evenly, stir at 30-40°C and 300-500r / min for 2-3 hours, filter, wash with anhydrous ethanol for 3-5 times, and dry at 50-60°C under vacuum conditions for 8-10 hours to obtain modified nano-silica; (4) Weigh 100-105 parts of modified polyvinyl chloride, 8-10 parts of modified nano-silica, 4-5 parts of dioctyl phthalate, 2-3 parts of dibutyltin dilaurate, 1-2 parts of stearic acid, and 1-2 parts of PE wax in parts by mass and place them in an internal mixer. Stir at 150-160°C and 500-600 r / min for 8-10 min, place them in a calender for calendering, let them stand at 50-60°C for 5-6 h after calendering, and cool them naturally to room temperature to obtain a wear-resistant and impact-resistant polymer floor.

[0007] As an optimization, the reaction process of the thiolation of carbamoylphenylboronic acid in step (1) is: .

[0008] As an optimization, the reaction process of the thiolated benzisothiazolinone in step (1) is: .

[0009] As an optimization, the preparation method of the pre-modified polyvinyl chloride in step (2) is as follows: polyvinyl chloride, a sodium hydroxide aqueous solution with a mass fraction of 9% to 11%, and anhydrous ethanol are placed in a hydrothermal autoclave in a mass ratio of 1:(2-3):(6-8), stirred at 80-90°C and 500-700 r / min for 3-4 hours, filtered, washed with deionized water for 3-5 times, and dried at 50-60°C under vacuum conditions for 8-10 hours to obtain the pre-modified polyvinyl chloride.

[0010] As an optimization, the model of the polyvinyl chloride is SG-8.

[0011] As an optimization, the preparation method of the pretreated nano-silica in step (3) is: nano-silica and anhydrous ethanol are mixed uniformly in a mass ratio of 1:(20~30), silane hydrolyzate is added in an amount of 8~10 times the mass of the nano-silica, the reaction is carried out at 50~60°C and 300~500r / min with stirring for 2~3h, filtered, washed with anhydrous ethanol for 3~5 times, and dried at 70~80°C under vacuum conditions for 8~10h to obtain the pretreated nano-silica.

[0012] As an optimization, the preparation method of the silane hydrolyzate is: 3-aminopropyltriethoxysilane and anhydrous ethanol are mixed evenly in a mass ratio of 1:(40~50), the pH is adjusted to 4~6 with a 1 mol / L oxalic acid aqueous solution, and the mixture is stirred at 10~30°C and 300~500r / min for 50~60min to prepare a silane hydrolyzate.

[0013] As an optimization, the model of the PE wax in step (4) is LPO100F.

[0014] As an optimization, the process parameters of the calendering molding in step (4) are: setting the calender temperature to 170-180°C, the calendering speed to 50-60m / min, and the pressure to 24-30MPa.

[0015] Compared with the prior art, the beneficial effects achieved by the present invention are: When preparing the wear-resistant and impact-resistant polymer floor, the present invention comprises the following steps: reacting 4-formyl chlorophenylboric acid and 3-mercapto-1-propylamine to obtain thiolated carbamoylphenylboric acid; reacting 1,2-benzisothiazolin-3-one and 3-chloro-1-propanethiol to obtain thiolated benzisothiazolinone; reacting polyvinyl chloride and sodium hydroxide to obtain pre-modified polyvinyl chloride; reacting pre-modified polyvinyl chloride, thiolated carbamoylphenylboric acid and thiolated benzisothiazolinone to obtain modified polyvinyl chloride. olefins; nano-silica and 3-aminopropyltriethoxysilane are reacted to obtain pretreated nano-silica; bis(oxiranylmethyl)phenyl phosphate and 1,5-diaminonaphthalene are polymerized and grown on pretreated nano-silica to obtain pre-modified nano-silica; pre-modified nano-silica and 4-formylchlorophenylboric acid are reacted to obtain modified nano-silica; modified polyvinyl chloride and modified nano-silica are kneaded and then calendered to obtain wear-resistant and impact-resistant polymer flooring.

[0016] Firstly, 4-formylchlorophenylboronic acid and 3-mercapto-1-propylamine are reacted to obtain thiolated carbamoylphenylboronic acid; 1,2-benzisothiazolin-3-one and 3-chloro-1-propanethiol are reacted to obtain thiolated benzisothiazolinone; polyvinyl chloride and sodium hydroxide are reacted to obtain pre-modified polyvinyl chloride, and a carbon-carbon double bond is introduced into the main chain of the pre-modified polyvinyl chloride molecule; the carbon-carbon double bond on the pre-modified polyvinyl chloride is reacted with the thiol groups on the thiolated carbamoylphenylboronic acid and the thiol groups on the thiolated benzisothiazolinone to undergo addition reaction. The modified polyvinyl chloride is prepared by introducing a benzisothiazolinone structure and a carbamoylphenylboronic acid structure into the side chain of the modified polyvinyl chloride molecule; benzisothiazolinone has a strong penetrating effect on the cell wall and cell membrane of microorganisms, and can enter the protein and other molecules containing the S element in the cell to act, so that the S atom in the benzisothiazolinone molecule is attacked by a nucleophilic agent, resulting in the SN bond breaking, and forming an SS bond with the receptor, thereby causing the normal physiological function of the microbial cell to be destroyed, and giving the microorganism a high wear resistance and impact resistance. The molecular floor has excellent antibacterial properties; the boric acid on the carbamoylphenylboronic acid structure can form a hexafluoroborane, forming a cross-linked network, inhibiting the relative slip between the polyvinyl chloride molecular chains, not easily torn by external shear force, reducing wear, and giving the wear-resistant and impact-resistant polymer floor excellent wear resistance; B and N on the carbamoylphenylboronic acid structure form a BN coordination structure, which is a weak bond. When the material is subjected to external force, the BN coordination structure will be the first to break and dissipate a large amount of energy. The BN coordination structure can be used as a "sacrificial bond" to improve the impact resistance of the wear-resistant and impact-resistant polymer floor; it is well known that the decomposition and dehydration of the hexafluoroborane often require the assistance of high temperature or water. However, there is a weak coordination structure between the -NH- on the carbamoylphenylboronic acid structure and the hexafluoroborane, which reduces the energy required for the conversion between the hexafluoroborane and boric acid, thereby promoting the decomposition and formation of the hexafluoroborane, so that the hexafluoroborane can undergo dynamic exchange reactions in air at room temperature, giving the wear-resistant and impact-resistant polymer floor excellent self-repairing properties.

[0017] Secondly, nano-silica and 3-aminopropyltriethoxysilane are reacted to obtain pretreated nano-silica; amino groups are introduced into the pretreated nano-silica, bis(oxiranylmethyl)phenyl phosphate and 1,5-diaminonaphthalene are polymerized and grown on the pretreated nano-silica, and 1,5-diaminonaphthalene is made excessive to obtain pre-modified nano-silica; phosphorus element, diaminonaphthalene and amino groups are introduced into the pre-modified nano-silica; phosphorus element can improve the flame retardant properties of wear-resistant and impact-resistant polymer flooring, diaminonaphthalene has thermal stability, and will release smoke and flame-retardant gases that inhibit combustion at high temperatures, further improving the flame retardant properties of wear-resistant and impact-resistant polymer flooring; the pre-modified nano-silica The amino group introduced on the surface reacts with the acyl chloride on 4-formyl chloride phenylboronic acid to obtain modified nano-silica, and carbamoyl phenylboronic acid is formed on the modified nano-silica, which reacts with carbamoyl phenylboronic acid introduced on the side chain of the polyvinyl chloride molecule to form boroxyhexacyclic ring, which participates in the cross-linking of the polyvinyl chloride. Nano-silica has a high specific surface area and excellent mechanical properties, and can improve the strength and hardness of the matrix resin. The nano-silica is modified to increase the compatibility of the nano-silica with the matrix resin, reduce the agglomeration of the nano-silica, and make the nano-silica uniformly dispersed in the matrix resin, so as to give full play to the reinforcing effect of the nano-silica and further improve the wear resistance of the wear-resistant and impact-resistant polymer floor. DETAILED DESCRIPTION

[0018] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0019] A preparation process of a wear-resistant and impact-resistant polymer floor, the preparation process of the wear-resistant and impact-resistant polymer floor comprising the following preparation steps: (1) Add 4-formyl chlorophenylboronic acid and 3-mercapto-1-propylamine in a molar ratio of 1:1 to tetrahydrofuran (8 times the mass of 4-formyl chlorophenylboronic acid), add triethylamine (0.03 times the mass of 4-formyl chlorophenylboronic acid), stir and react at 10°C and 300 r / min for 3 hours, and dry at 50°C for 8 hours under vacuum conditions to obtain thiolated aminoformylphenylboronic acid; add 1,2-benzisothiazolin-3-one and 3-chloro-1-propanethiol in a molar ratio of 1:1 to tetrahydrofuran (8 times the mass of 1,2-benzisothiazolin-3-one), add triethylamine (0.03 times the mass of 1,2-benzisothiazolin-3-one), stir and react at 40°C and 300 r / min for 3 hours, and dry at 50°C for 8 hours under vacuum conditions to obtain thiolated benzisothiazolinone; (2) Polyvinyl chloride, 9% sodium hydroxide aqueous solution and anhydrous ethanol were placed in a hydrothermal autoclave in a mass ratio of 1:2:6, stirred at 80°C and 500 r / min for 4 h, filtered, washed with deionized water for 3 times, and dried at 50°C for 10 h under vacuum conditions to obtain pre-modified polyvinyl chloride; pre-modified polyvinyl chloride, thiolated carbamoylphenylboronic acid, thiolated benzisothiazolinone, azobisisobutyronitrile and N,N-dimethylformamide were mixed evenly in a mass ratio of 1:0.3:0.2:0.03:10, stirred at 70°C and 300 r / min for 4 h, and dried at 50°C for 10 h under vacuum conditions to obtain modified polyvinyl chloride; (3) 3-aminopropyltriethoxysilane and anhydrous ethanol were mixed at a mass ratio of 1:40, the pH was adjusted to 4 with a 1 mol / L oxalic acid aqueous solution, and the mixture was stirred at 10°C and 300 r / min for 60 min to prepare a silane hydrolyzate; nano-silica and anhydrous ethanol were mixed at a mass ratio of 1:20, 8 times the mass of the nano-silica was added to the silane hydrolyzate, and the mixture was stirred at 50°C and 300 r / min for 3 h, filtered, washed with anhydrous ethanol for 3 times, and dried at 70°C under vacuum for 10 h to prepare pretreated nano-silica; bis(oxiranylmethyl)phenyl phosphate and 1,5-diaminonaphthalene were added at a molar ratio of 1:1.2 To toluene with a mass of 12 times that of bis(oxiranylmethyl)phenyl phosphate, add pretreated nano-silica with a mass of 0.6 times that of bis(oxiranylmethyl)phenyl phosphate, stir and react at 50°C, 300r / min for 6h, filter, wash with anhydrous ethanol 3 times, and dry at 50°C for 10h under vacuum conditions to obtain pre-modified nano-silica; mix the pre-modified nano-silica, 4-formylchlorophenylboronic acid, triethylamine, and tetrahydrofuran in a mass ratio of 1:2:0.03:10, stir and react at 30°C, 300r / min for 3h, filter, wash with anhydrous ethanol 3 times, and dry at 50°C for 10h under vacuum conditions to obtain modified nano-silica; (4) Weigh 100 parts of modified polyvinyl chloride, 8 parts of modified nano-silica, 4 parts of dioctyl phthalate, 2 parts of dibutyltin dilaurate, 1 part of stearic acid, and 1 part of PE wax by mass, place them in an internal mixer, stir at 150°C and 500 r / min for 10 min, place them in a calender, set the calender temperature to 170°C, the calender speed to 50 m / min, and the pressure to 24 MPa, stand at 50°C for 6 h after calendering, and cool naturally to room temperature to obtain a wear-resistant and impact-resistant polymer floor.

[0020] A preparation process of a wear-resistant and impact-resistant polymer floor, the preparation process of the wear-resistant and impact-resistant polymer floor comprising the following preparation steps: (1) Add 4-formyl chlorophenylboronic acid and 3-mercapto-1-propylamine in a molar ratio of 1:1 to tetrahydrofuran (9 times the mass of 4-formyl chlorophenylboronic acid), add triethylamine (0.04 times the mass of 4-formyl chlorophenylboronic acid), stir at 20°C and 400 r / min for 2.5 h, and dry at 55°C for 7.5 h under vacuum conditions to obtain thiolated aminoformylphenylboronic acid; add 1,2-benzisothiazolin-3-one and 3-chloro-1-propanethiol in a molar ratio of 1:1 to tetrahydrofuran (9 times the mass of 1,2-benzisothiazolin-3-one), add triethylamine (0.04 times the mass of 1,2-benzisothiazolin-3-one), stir at 45°C and 400 r / min for 2.5 h, and dry at 55°C for 7.5 h under vacuum conditions to obtain thiolated benzisothiazolinone; (2) Polyvinyl chloride, 10% sodium hydroxide aqueous solution, and anhydrous ethanol were placed in a hydrothermal autoclave in a mass ratio of 1:2.5:7, stirred at 85°C and 600 r / min for 3.5 h, filtered, washed with deionized water 4 times, and dried at 55°C for 9 h under vacuum conditions to obtain pre-modified polyvinyl chloride; pre-modified polyvinyl chloride, thiolated carbamoylphenylboronic acid, thiolated benzisothiazolinone, azobisisobutyronitrile, and N,N-dimethylformamide were mixed evenly in a mass ratio of 1:0.35:0.25:0.04:11, stirred at 75°C and 400 r / min for 3.5 h, and dried at 55°C for 9 h under vacuum conditions to obtain modified polyvinyl chloride; (3) 3-aminopropyltriethoxysilane and anhydrous ethanol were mixed at a mass ratio of 1:45, the pH was adjusted to 5 with a 1 mol / L oxalic acid aqueous solution, and the mixture was stirred at 20°C and 400 r / min for 55 min to prepare a silane hydrolyzate; nano-silica and anhydrous ethanol were mixed at a mass ratio of 1:25, 9 times the mass of nano-silica was added with silane hydrolyzate, and the mixture was stirred at 55°C and 400 r / min for 2.5 h, filtered, washed with anhydrous ethanol for 4 times, and dried at 75°C under vacuum for 9 h to prepare pretreated nano-silica; bis(oxiranylmethyl)phenyl phosphate and 1,5-diaminonaphthalene were added at a molar ratio of 1:1.25 To toluene with a mass of 13 times that of bis(oxiranylmethyl)phenyl phosphate, add pretreated nano-silica with a mass of 0.7 times that of bis(oxiranylmethyl)phenyl phosphate, stir and react at 55°C, 400r / min for 5h, filter, wash with anhydrous ethanol 4 times, and dry at 55°C for 9h under vacuum conditions to obtain pre-modified nano-silica; mix the pre-modified nano-silica, 4-formylchlorophenylboronic acid, triethylamine, and tetrahydrofuran in a mass ratio of 1:2.5:0.04:11, stir and react at 35°C, 400r / min for 2.5h, filter, wash with anhydrous ethanol 4 times, and dry at 55°C for 9h under vacuum conditions to obtain modified nano-silica; (4) Weigh 102.5 parts of modified polyvinyl chloride, 9 parts of modified nano-silica, 4.5 parts of dioctyl phthalate, 2.5 parts of dibutyltin dilaurate, 1.5 parts of stearic acid, and 1.5 parts of PE wax in parts by mass, place them in an internal mixer, stir at 155°C and 550 r / min for 9 min, place them in a calender, set the calender temperature to 175°C, the calender speed to 55 m / min, and the pressure to 27 MPa, and after calendering, let it stand at 55°C for 5.5 h, and cool naturally to room temperature to obtain a wear-resistant and impact-resistant polymer floor.

[0021] A preparation process of a wear-resistant and impact-resistant polymer floor, the preparation process of the wear-resistant and impact-resistant polymer floor comprising the following preparation steps: (1) Add 4-formyl chlorophenylboronic acid and 3-mercapto-1-propylamine in a molar ratio of 1:1 to tetrahydrofuran (10 times the mass of 4-formyl chlorophenylboronic acid), add triethylamine (0.05 times the mass of 4-formyl chlorophenylboronic acid), stir and react at 30°C and 500 r / min for 2 hours, and dry at 60°C for 7 hours under vacuum conditions to obtain thiolated aminoformylphenylboronic acid; add 1,2-benzisothiazolin-3-one and 3-chloro-1-propanethiol in a molar ratio of 1:1 to tetrahydrofuran (10 times the mass of 1,2-benzisothiazolin-3-one), add triethylamine (0.05 times the mass of 1,2-benzisothiazolin-3-one), stir and react at 50°C and 500 r / min for 2 hours, and dry at 60°C for 7 hours under vacuum conditions to obtain thiolated benzisothiazolinone; (2) Polyvinyl chloride, sodium hydroxide aqueous solution with a mass fraction of 11%, and anhydrous ethanol were placed in a hydrothermal autoclave in a mass ratio of 1:3:8, stirred at 90°C and 700 r / min for 3 h, filtered, washed with deionized water 5 times, and dried at 60°C for 8 h under vacuum conditions to obtain pre-modified polyvinyl chloride; pre-modified polyvinyl chloride, thiolated carbamoylphenylboronic acid, thiolated benzisothiazolinone, azobisisobutyronitrile, and N,N-dimethylformamide were mixed evenly in a mass ratio of 1:0.4:0.3:0.05:12, stirred at 80°C and 500 r / min for 3 h, and dried at 60°C for 8 h under vacuum conditions to obtain modified polyvinyl chloride; (3) 3-aminopropyltriethoxysilane and anhydrous ethanol were mixed at a mass ratio of 1:50, the pH was adjusted to 6 with a 1 mol / L oxalic acid aqueous solution, and the mixture was stirred at 30°C and 500 r / min for 50 min to prepare a silane hydrolyzate; nano-silica and anhydrous ethanol were mixed at a mass ratio of 1:30, 10 times the mass of nano-silica was added to the silane hydrolyzate, and the mixture was stirred at 60°C and 500 r / min for 2 h, filtered, washed with anhydrous ethanol for 5 times, and dried at 80°C under vacuum for 8 h to prepare pretreated nano-silica; bis(oxiranylmethyl)phenyl phosphate and 1,5-diaminonaphthalene were added at a molar ratio of 1:1.3 The pre-modified nano-silica was prepared by mixing the pre-modified nano-silica with 4-formyl chlorophenylboronic acid, triethylamine and tetrahydrofuran in a mass ratio of 1:3:0.05:12, stirring at 40°C and 500 r / min for 2 hours, filtering, washing with anhydrous ethanol for 5 times, and drying at 60°C for 8 hours under vacuum conditions to obtain the pre-modified nano-silica. The pre-modified nano-silica, 4-formyl chlorophenylboronic acid, triethylamine and tetrahydrofuran were uniformly mixed in a mass ratio of 1:3:0.05:12, stirring at 40°C and 500 r / min for 2 hours, filtering, washing with anhydrous ethanol for 5 times, and drying at 60°C for 8 hours under vacuum conditions to obtain the modified nano-silica. (4) Weigh 105 parts of modified polyvinyl chloride, 10 parts of modified nano-silica, 5 parts of dioctyl phthalate, 3 parts of dibutyltin dilaurate, 2 parts of stearic acid, and 2 parts of PE wax in parts by mass, place them in an internal mixer, stir at 160°C and 600 r / min for 8 min, place them in a calender, set the calender temperature to 180°C, the calender speed to 60 m / min, and the pressure to 30 MPa, and after calendering, let it stand at 60°C for 5 h, and cool naturally to room temperature to obtain a wear-resistant and impact-resistant polymer floor.

[0022] Comparative Example 1: The difference between the preparation process of the wear-resistant and impact-resistant polymer floor of Comparative Example 1 and Example 2 lies in the difference between step (1) and step (2). Step (1) is modified as follows: 1,2-benzisothiazolin-3-one and 3-chloro-1-propanethiol are added in a molar ratio of 1:1 to tetrahydrofuran (9 times the mass of 1,2-benzisothiazolin-3-one), and triethylamine (0.04 times the mass of 1,2-benzisothiazolin-3-one) is added, and the mixture is stirred at 45°C and 400 r / min for 2.5 h. The mixture is dried at 55°C for 7.5 h under vacuum to obtain thiolated benzisothiazolinone; step (2) is modified as follows: polyvinyl chloride is added to the mixture; The pre-modified polyvinyl chloride was prepared by mixing the pre-modified polyvinyl chloride, the mercapto-benzisothiazolinone, the azobisisobutyronitrile and the N,N-dimethylformamide in a mass ratio of 1:0.25:0.04:11, stirring and reacting at 75°C, 400r / min for 3.5h, and drying at 55°C for 9h under vacuum conditions. The remaining steps were the same as those in Example 2.

[0023] Comparative Example 2: The preparation process of the wear-resistant and impact-resistant polymer floor of Comparative Example 2 is different from that of Example 2 in that step (1) and step (2) are different. Step (1) is modified as follows: 4-formyl chlorophenylboric acid and 3-mercapto-1-propylamine are added in a molar ratio of 1:1 to tetrahydrofuran (9 times the mass of 4-formyl chlorophenylboric acid), and triethylamine (0.04 times the mass of 4-formyl chlorophenylboric acid) is added, and the mixture is stirred at 20° C. and 400 r / min for 2.5 h. The mixture is dried at 55° C. for 7.5 h under vacuum conditions to obtain thiolated carbamoylphenylboric acid; step (2) is modified as follows: polyvinyl chloride and 1% by mass of ... 0% sodium hydroxide aqueous solution and anhydrous ethanol are placed in a hydrothermal autoclave at a mass ratio of 1:2.5:7, stirred at 85°C and 600r / min for 3.5h, filtered, washed with deionized water 4 times, and dried at 55°C for 9h under vacuum to obtain pre-modified polyvinyl chloride; pre-modified polyvinyl chloride, thiolated carbamoylphenylboronic acid, azobisisobutyronitrile, and N,N-dimethylformamide are mixed uniformly at a mass ratio of 1:0.35:0.04:11, stirred at 75°C and 400r / min for 3.5h, and dried at 55°C for 9h under vacuum to obtain modified polyvinyl chloride. The remaining steps are the same as those in Example 2.

[0024] Comparative Example 3: The preparation process of the wear-resistant and impact-resistant polymer floor of Comparative Example 3 is different from that of Example 2 only in step (1) and step (2). Step (1) is modified as follows: 1,2-benzisothiazolin-3-one and 3-chloro-1-propanethiol are added in a molar ratio of 1:1 to tetrahydrofuran (9 times the mass of 1,2-benzisothiazolin-3-one), and triethylamine (0.04 times the mass of 1,2-benzisothiazolin-3-one) is added, and the mixture is stirred at 45°C and 400 r / min for 2.5 h, and dried at 55°C for 7.5 h under vacuum conditions to obtain thiolated benzisothiazolinone; step (2) is modified as follows: polyvinyl chloride, mass fraction 10% sodium hydroxide aqueous solution and anhydrous ethanol are placed in a hydrothermal autoclave in a mass ratio of 1:2.5:7, stirred at 85°C and 600r / min for 3.5h, filtered, washed with deionized water 4 times, and dried at 55°C for 9h under vacuum conditions to obtain pre-modified polyvinyl chloride; pre-modified polyvinyl chloride, 4-mercaptophenylboric acid, mercaptobenzoisothiazolinone, azobisisobutyronitrile, and N,N-dimethylformamide are mixed in a mass ratio of 1:0.35:0.25:0.04:11, stirred at 75°C and 400r / min for 3.5h, and dried at 55°C for 9h under vacuum conditions to obtain modified polyvinyl chloride. The remaining steps are the same as those in Example 2.

[0025] Comparative Example 4: The preparation process of the wear-resistant and impact-resistant polymer floor of Comparative Example 4 is different from that of Example 2 in that step (3) is not performed, and step (4) is modified as follows: 102.5 parts of modified polyvinyl chloride, 9 parts of nano-silicon dioxide, 4.5 parts of dioctyl phthalate, 2.5 parts of dibutyltin dilaurate, 1.5 parts of stearic acid, and 1.5 parts of PE wax are weighed by mass and placed in an internal mixer, stirred at 155° C. and 550 r / min for 9 minutes, placed in a calender, and the calender temperature is set to 175° C., the calender speed is set to 55 m / min, and the pressure is set to 27 MPa. After calendering, the mixture is allowed to stand at 55° C. for 5.5 hours, and naturally cooled to room temperature to obtain a wear-resistant and impact-resistant polymer floor. The remaining steps are the same as those of Example 2.

[0026] Test Example 1 Impact resistance test Test method: The impact strength of the examples and comparative examples was tested on an impact tester according to GB / T1043. The results are shown in Table 1.

[0027] Table 1 Impact strength (kJ / m2) Impact strength (kJ / m2) Example 1 43.2 Comparative Example 1 28.2 Example 2 44.1 Comparative Example 2 42.2 Example 3 42.7 Comparative Example 3 27.1 Comparative Example 4 41.9 From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 4 in Table 1, it can be found that the wear-resistant and impact-resistant polymer floor prepared by the present invention has good impact resistance.

[0028] By comparison, the impact strength of Examples 1 to 3 is greater than that of Comparative Examples 1 and 3, indicating that 4-formylchlorophenylboronic acid and 3-mercapto-1-propylamine are reacted to obtain thiolated carbamoylphenylboronic acid; polyvinyl chloride and sodium hydroxide are reacted to obtain pre-modified polyvinyl chloride, and a carbon-carbon double bond is introduced into the main chain of the pre-modified polyvinyl chloride molecule; the carbon-carbon double bond on the pre-modified polyvinyl chloride is reacted with the thiol group on the thiolated carbamoylphenylboronic acid to obtain modified polyvinyl chloride, and a carbamoylphenylboronic acid structure is introduced into the side chain of the modified polyvinyl chloride molecule; B and N on the carbamoylphenylboronic acid structure form a BN coordination structure, which is a weak bond. When the material is subjected to external force, the BN coordination structure will be the first to break and dissipate a large amount of energy. The BN coordination structure can be used as a "sacrificial bond" to improve the impact resistance of the wear-resistant and impact-resistant polymer floor.

[0029] Test Example 2 Wear resistance test Test method: The wear resistance of the embodiments and comparative examples was tested using the FRICK-TABER falling sand method, and the volume loss of each specimen after 100 turns of wear was calculated. The results are shown in Table 2 Table 2 100r volume loss (mm3) 100r volume loss (mm3) Example 1 1.21 Comparative Example 1 5.33 Example 2 1.06 Comparative Example 2 1.28 Example 3 1.12 Comparative Example 3 1.32 Comparative Example 4 4.92 From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 4 in Table 2, it can be found that the wear-resistant and impact-resistant polymer floor prepared by the present invention has good wear resistance.

[0030] By comparison, the 100r volume loss of Examples 1 to 3 is less than the 100r volume loss of Comparative Example 1, indicating that 4-formylchlorophenylboronic acid and 3-mercapto-1-propylamine are reacted to obtain thiolated carbamoylphenylboronic acid; polyvinyl chloride and sodium hydroxide are reacted to obtain pre-modified polyvinyl chloride, and a carbon-carbon double bond is introduced into the main chain of the pre-modified polyvinyl chloride molecule; the carbon-carbon double bond on the pre-modified polyvinyl chloride is reacted with the thiol group on the thiolated carbamoylphenylboronic acid to obtain modified polyvinyl chloride, and a carbamoylphenylboronic acid structure is introduced into the side chain of the modified polyvinyl chloride molecule; the boric acid on the carbamoylphenylboronic acid structure can form a hexacyclic borane to form a cross-linked network, thereby inhibiting the relative slip between polyvinyl chloride molecular chains, making it not easily torn by external shear force, reducing wear, and giving the wear-resistant and impact-resistant polymer floor excellent wear resistance.

[0031] By comparison, the 100r volume loss of Examples 1 to 3 is less than the 100r volume loss of Comparative Example 4, indicating that the pretreated nano-silica is prepared by reacting nano-silica and 3-aminopropyltriethoxysilane; an amino group is introduced into the pretreated nano-silica, bis(oxiranylmethyl)phenyl phosphate and 1,5-diaminonaphthalene are polymerized and grown on the pretreated nano-silica, and 1,5-diaminonaphthalene is made excessive to prepare pre-modified nano-silica; the amino group introduced into the pre-modified nano-silica is reacted with the acyl chloride on 4-formylchlorophenylboronic acid to prepare modified nano-silica, and Carbamoylphenylboric acid is formed on the modified nano-silica, which reacts with the carbamoylphenylboric acid introduced on the side chain of the polyvinyl chloride molecule to form boroxyhexacyclic ring, which participates in the cross-linking of the polyvinyl chloride. Nano-silica has a high specific surface area and excellent mechanical properties, and can improve the strength and hardness of the matrix resin. The nano-silica is modified to increase the compatibility of the nano-silica with the matrix resin, reduce the agglomeration of the nano-silica, and make the nano-silica evenly dispersed in the matrix resin, so as to give full play to the reinforcing effect of the nano-silica and further improve the wear resistance of the wear-resistant and impact-resistant polymer floor.

[0032] Test Example 3 Self-healing performance test Test method: According to GB / T1040.1, the embodiment and the comparative example were prepared into standard specimens, and their original tensile strength was tested with a tensile machine. Then, a 2mm deep and 20mm long crack was cut from the middle of the unstretched original specimen, placed in a mold, and left to stand at room temperature for 24 hours to obtain the repaired specimen. The tensile strength was tested with a tensile machine. The self-repair rate of the embodiment and the comparative example before and after repair was calculated, and the self-repair rate = (tensile strength of the specimen after repair / original tensile strength of the specimen) × 100%. The results are shown in Table 3.

[0033] Table 3 Self-repair rate (%) Self-repair rate (%) Example 1 95.97 Comparative Example 1 52.23 Example 2 96.24 Comparative Example 2 95.62 Example 3 96.13 Comparative Example 3 83.29 Comparative Example 4 95.58 From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 4 in Table 3, it can be found that the wear-resistant and impact-resistant polymer floor prepared by the present invention has good self-repairing performance.

[0034] By comparison, the self-repairing rates of Examples 1 to 3 are greater than those of Comparative Examples 1 and 3, and the self-repairing rate of Comparative Example 3 is greater than that of Comparative Example 1, indicating that 4-formylchlorophenylboronic acid and 3-mercapto-1-propylamine are reacted to obtain thiolated carbamoylphenylboronic acid; polyvinyl chloride and sodium hydroxide are reacted to obtain pre-modified polyvinyl chloride, and a carbon-carbon double bond is introduced into the main chain of the pre-modified polyvinyl chloride molecule; the carbon-carbon double bond on the pre-modified polyvinyl chloride is reacted with the thiol group on the thiolated carbamoylphenylboronic acid to obtain modified polyvinyl chloride, and the modified polyvinyl chloride is obtained by reacting the carbon-carbon double bond on the pre-modified polyvinyl chloride with the thiol group on the thiolated carbamoylphenylboronic acid. The carbamoylphenylboronic acid structure is introduced into the side chain of the molecule; the boric acid on the carbamoylphenylboronic acid structure can form boroxane to form a cross-linked network; it is well known that the decomposition and dehydration of boroxane often require the assistance of high temperature or water, but there is a weak coordination structure between the -NH- on the carbamoylphenylboronic acid structure and the boroxane, which reduces the energy required for the conversion between the boroxane and boric acid, thereby promoting the decomposition and formation of the boroxane, so that the boroxane can undergo a dynamic exchange reaction in the air at room temperature, giving the wear-resistant and impact-resistant polymer floor excellent self-healing properties.

[0035] Test Example 4 Antimicrobial performance testing Test method: The examples and comparative examples were cut into 10 mm × 10 mm × 5 mm samples and sterilized by ultraviolet irradiation for 3 h; the Escherichia coli strains were activated and prepared to a concentration of 3 × 10 4 cfu / ml bacterial suspension; put the sample into the bacterial suspension, shake at 300r / min for 5min at room temperature, take 1ml of the bacterial suspension and dilute it to 100 times, take 1ml of the diluted bacterial suspension and inoculate it into agar medium, culture it at 37℃ for 16h, count the colonies according to the method in GB / T15979, and calculate the antibacterial rate. The results are shown in Table 4.

[0036] Table 4 Antibacterial rate (%) Antibacterial rate (%) Example 1 99.73 Comparative Example 1 99.71 Example 2 99.85 Comparative Example 2 72.58 Example 3 99.81 Comparative Example 3 99.69 Comparative Example 4 99.64 From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 4 in Table 4, it can be found that the wear-resistant and impact-resistant polymer floor prepared by the present invention has good antibacterial properties.

[0037] By comparison, the antibacterial rates of Examples 1 to 3 are greater than that of Comparative Example 2, indicating that 1,2-benzisothiazolin-3-one and 3-chloro-1-propanethiol are reacted to obtain thiolated benzisothiazolinone; polyvinyl chloride and sodium hydroxide are reacted to obtain pre-modified polyvinyl chloride, and a carbon-carbon double bond is introduced into the main chain of the pre-modified polyvinyl chloride molecule; the carbon-carbon double bond on the pre-modified polyvinyl chloride is subjected to an addition reaction with the thiol group on the thiolated benzisothiazolinone to obtain modified polyvinyl chloride, and a benzisothiazolinone structure is introduced into the side chain of the modified polyvinyl chloride molecule; benzisothiazolinone has a strong penetrating effect on microbial cell walls and cell membranes, and can enter into the cells to act on proteins and other molecules containing S elements, so that the S atom in the benzisothiazolinone molecule is attacked by a nucleophilic agent, resulting in the breaking of the SN bond, and forming an SS bond with the receptor, thereby causing the normal physiological function of the microbial cell to be destroyed, thereby giving the wear-resistant and impact-resistant polymer floor excellent antibacterial properties.

[0038] Test Example 5 Flame retardant performance test Test method: The examples and comparative examples were prepared into standard specimens according to GB / T2406.2, and the limiting oxygen index of the standard specimens was tested. The results are shown in Table 5.

[0039] Table 5 Limiting oxygen index (%) Limiting oxygen index (%) Example 1 39.27 Comparative Example 1 38.75 Example 2 40.15 Comparative Example 2 39.16 Example 3 39.94 Comparative Example 3 38.92 Comparative Example 4 28.74 From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 4 in Table 5, it can be found that the wear-resistant and impact-resistant polymer floor prepared by the present invention has good flame retardant properties.

[0040] By comparison, the limiting oxygen index of Examples 1 to 3 is greater than that of Comparative Example 4, indicating that pretreated nano-silica is prepared by reacting nano-silica and 3-aminopropyltriethoxysilane; amino groups are introduced into the pretreated nano-silica, bis(oxiranylmethyl)phenyl phosphate and 1,5-diaminonaphthalene are polymerized and grown on the pretreated nano-silica, and 1,5-diaminonaphthalene is excessively added to prepare pre-modified nano-silica; phosphorus element and diaminonaphthalene are introduced into the pre-modified nano-silica; phosphorus element can improve the flame retardant properties of the wear-resistant and impact-resistant polymer floor, and diaminonaphthalene has thermal stability, and will release smoke and flame-retardant gases that inhibit combustion at high temperatures, further improving the flame retardant properties of the wear-resistant and impact-resistant polymer floor.

[0041] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A wear-resistant and impact-resistant polymer floor, characterized in that: The wear-resistant and impact-resistant polymer floor is prepared by reacting pre-modified polyvinyl chloride, mercaptolated carbamoylphenylboronic acid and mercaptolated benzisothiazolinone to obtain modified polyvinyl chloride; reacting pre-modified nano-silica and 4-formyl chloride phenylboronic acid to obtain modified nano-silica; and kneading the modified polyvinyl chloride and the modified nano-silica and then calendering to obtain the floor. The thiolated carbamoylphenylboronic acid is prepared by reacting 4-formylchlorophenylboronic acid and 3-mercapto-1-propylamine; The thiolated benzisothiazolinone is prepared by reacting 1,2-benzisothiazolin-3-one and 3-chloro-1-propanethiol; The pre-modified polyvinyl chloride is prepared by reacting polyvinyl chloride and sodium hydroxide; The pre-modified nano-silica is prepared by polymerizing bis(oxiranylmethyl)phenyl phosphate and 1,5-diaminonaphthalene on pre-treated nano-silica. The pretreated nano silicon dioxide is prepared by reacting nano silicon dioxide and 3-aminopropyltriethoxysilane.

2. A process for preparing a wear-resistant and impact-resistant polymer floor, characterized in that: The preparation process of the wear-resistant and impact-resistant polymer floor comprises the following preparation steps: (1) Add 4-formyl chlorophenylboronic acid and 3-mercapto-1-propylamine in a molar ratio of 1:1 to tetrahydrofuran (8 to 10 times the mass of 4-formyl chlorophenylboronic acid), add triethylamine (0.03 to 0.05 times the mass of 4-formyl chlorophenylboronic acid), stir at 10 to 30°C and 300 to 500 r / min for 2 to 3 hours, and dry at 50 to 60°C under vacuum for 7 to 8 hours to obtain thiolated carbamoylphenylboronic acid; Add 1,2-benzisothiazolin-3-one and 3-chloro-1-propanethiol in a molar ratio of 1:1 to tetrahydrofuran (8 to 10 times the mass of 1,2-benzisothiazolin-3-one), add triethylamine (0.03 to 0.05 times the mass of 1,2-benzisothiazolin-3-one), stir at 40 to 50°C and 300 to 500 r / min for 2 to 3 hours, and dry at 50 to 60°C under vacuum for 7 to 8 hours to obtain thiolated benzisothiazolinone; (2) Pre-modified polyvinyl chloride, thiolated carbamoylphenylboronic acid, thiolated benzisothiazolinone, azobisisobutyronitrile, and N,N-dimethylformamide are mixed uniformly in a mass ratio of 1:(0.3-0.4):(0.2-0.3):(0.03-0.05):(10-12), stirred at 70-80°C and 300-500 r / min for 3-4 hours, and dried at 50-60°C under vacuum conditions for 8-10 hours to obtain modified polyvinyl chloride; (3) Add bis(oxiranylmethyl)phenyl phosphate and 1,5-diaminonaphthalene in a molar ratio of 1:(1.2-1.3) to toluene with a mass of 12-14 times that of bis(oxiranylmethyl)phenyl phosphate, add pretreated nano-silica with a mass of 0.6-0.8 times that of bis(oxiranylmethyl)phenyl phosphate, stir at 50-60°C and 300-500 r / min for 4-6 hours, filter, wash with anhydrous ethanol 3-5 times, and vacuum at 50-60°C. Dry at 60°C for 8-10 hours to obtain pre-modified nano-silica; mix pre-modified nano-silica, 4-formylchlorophenylboronic acid, triethylamine and tetrahydrofuran in a mass ratio of 1:(2-3):(0.03-0.05):(10-12) evenly, stir at 30-40°C and 300-500r / min for 2-3 hours, filter, wash with anhydrous ethanol for 3-5 times, and dry at 50-60°C under vacuum conditions for 8-10 hours to obtain modified nano-silica; (4) Weigh 100-105 parts of modified polyvinyl chloride, 8-10 parts of modified nano-silica, 4-5 parts of dioctyl phthalate, 2-3 parts of dibutyltin dilaurate, 1-2 parts of stearic acid, and 1-2 parts of PE wax in parts by mass and place them in an internal mixer. Stir at 150-160°C and 500-600 r / min for 8-10 min, place them in a calender for calendering, let them stand at 50-60°C for 5-6 h after calendering, and cool them naturally to room temperature to obtain a wear-resistant and impact-resistant polymer floor.

3. The process for preparing the wear-resistant and impact-resistant polymer floor according to claim 2, characterized in that: The preparation method of the pre-modified polyvinyl chloride in step (2) is as follows: polyvinyl chloride, a sodium hydroxide aqueous solution with a mass fraction of 9% to 11%, and anhydrous ethanol are placed in a hydrothermal kettle in a mass ratio of 1:(2-3):(6-8), stirred at 80-90°C and 500-700 r / min for 3-4 hours, filtered, washed with deionized water for 3-5 times, and dried at 50-60°C under vacuum conditions for 8-10 hours to obtain the pre-modified polyvinyl chloride.

4. The process for preparing the wear-resistant and impact-resistant polymer floor according to claim 3, characterized in that: The model of the polyvinyl chloride is SG-8.

5. The process for preparing the wear-resistant and impact-resistant polymer floor according to claim 2, characterized in that: The preparation method of the pretreated nano-silica in step (3) is as follows: nano-silica and anhydrous ethanol are uniformly mixed in a mass ratio of 1:(20-30), silane hydrolyzate is added in an amount of 8-10 times the mass of the nano-silica, the mixture is stirred at 50-60°C and 300-500 r / min for 2-3 hours, filtered, washed with anhydrous ethanol for 3-5 times, and dried at 70-80°C under vacuum conditions for 8-10 hours to obtain the pretreated nano-silica.

6. The process for preparing the wear-resistant and impact-resistant polymer floor according to claim 5, characterized in that: The preparation method of the silane hydrolyzate is as follows: 3-aminopropyltriethoxysilane and anhydrous ethanol are uniformly mixed in a mass ratio of 1:(40-50), the pH value is adjusted to 4-6 with a 1 mol / L oxalic acid aqueous solution, and the silane hydrolyzate is prepared by stirring at 10-30° C. and 300-500 r / min for 50-60 min.

7. The process for preparing the wear-resistant and impact-resistant polymer floor according to claim 2, characterized in that: The model of the PE wax in step (4) is LPO100F.

8. The process for preparing the wear-resistant and impact-resistant polymer floor according to claim 2, characterized in that: The process parameters of the calendering molding in step (4) are: setting the calender temperature to 170-180°C, the calendering speed to 50-60m / min, and the pressure to 24-30MPa.