Moisture power generation gel material as well as preparation method and application thereof
The moisture-generating gel material prepared by blending polymer PVA, single-layer graphene and LiCl is solved, and the problem of insufficient selection of moisture-generating materials and process improvement is achieved, and the stable power generation performance and humidity response within a wide humidity range is achieved. Capability, suitable for humidity detection and flexible self-powered devices.
Patent Information
- Application Number
- CN202411181935.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-06
AI Technical Summary
The selection of moisture power generation materials and imperfect process improvements limit the further application and performance stability of moisture power generation technology, and is difficult to respond effectively especially when environmental humidity changes.
The moisture-generating gel material prepared by blending polymer PVA, single-layer graphene and LiCl is achieved through a simple preparation method to achieve humidity power generation behavior within the range of relative humidity 40%-98%, combining the conductivity of single-layer graphene and the hygroscopicity of LiCl, forming a stable moisture-generating gel material.
It realizes stable power generation performance in a wide humidity range, with a maximum average power generation voltage of up to 0.632V, which can effectively respond to changes in environmental humidity. It is suitable for humidity detection, breathing monitoring and flexible self-powered devices.
Smart Images

Figure CN119081324A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of wet gas power generation, and in particular to a wet gas power generation gel material and a preparation method and application thereof. Background Art
[0002] There are abundant energy sources in the natural environment, such as light energy, mechanical energy and thermal energy. These energy sources have great development potential, but due to their wide dispersion and difficulty in centralization, traditional energy conversion technologies are often difficult to use effectively. In recent years, researchers have proposed a series of new energy generation technologies that aim to use different energy sources in the environment to generate electricity. For example, photovoltaic power generation uses photoelectric functional materials to generate electricity under light stimulation; piezoelectric power generation uses piezoelectric materials to generate potential difference under mechanical force; triboelectric power generation and thermal power generation use static electricity generated by friction and potential difference generated by temperature difference to generate electricity respectively.
[0003] In 2015, wet gas power generation was first proposed and reported, and has gradually become one of the hot spots in the field of new energy and monitoring. The core concept of wet gas power generation technology is to collect energy based on the diffusion of water molecules, realizing efficient energy conversion from chemical potential to electrical output. At present, there are two main explanations for the principle of wet gas power generation: the ion diffusion model and the streaming potential model. The former generates electricity by generating an ion concentration difference to form an ion gradient, while the latter mainly generates a double layer through solid-liquid interaction and generates a net charge through liquid movement. However, since wet gas power generation is in its early stages, there are fewer choices for wet gas power generation materials and imperfect improvement processes, which greatly limit the further application of wet gas power generation.
[0004] The performance of wet gas power generation is affected by the ambient humidity. Similarly, the electrical performance of the device can also reflect the changes in ambient humidity. Therefore, a sensitive humidity detector can be designed based on this feature of wet gas power generation. At the same time, human breathing is also accompanied by short-term and drastic changes in humidity, and the wet gas power generation device also responds to this. Summary of the invention
[0005] Purpose of the invention: In view of the problems existing in the prior art, the present invention provides a moisture power generation gel material with good stability. The present invention also provides a preparation method and application of the moisture power generation gel material. The method is simple to prepare and the conditions are mild. It can realize moisture power generation behavior in a wide humidity range of 40%-98% relative humidity. The material of the present invention is used in devices such as humidity detection, breathing monitoring, and flexible self-power supply.
[0006] Technical solution: The wet gas power generation gel material described in the present invention comprises PVA, single-layer graphene and LiCl, wherein the mass percentage of the single-layer graphene to PVA is 0.5% to 1.5%, and the mass percentage of LiCl to PVA is 10% to 50%.
[0007] Preferably, the PVA is PVA 1799 type.
[0008] Most preferably, the mass percentage of the single-layer graphene to PVA is 1%, and the mass ratio of LiCl to PVA is 15%-25%.
[0009] The gel material is prepared by the following method: PVA is poured into a solvent, heated and stirred until the PVA is completely dissolved and becomes transparent, thereby obtaining a colorless and transparent PVA sol; after standing and cooling, a single-layer graphene is added, heated and stirred until uniformly dispersed, thereby obtaining a PVA / single-layer graphene mixed sol PG; after standing and cooling, LiCl is added, heated and stirred until uniformly dispersed, thereby obtaining a PVA / single-layer graphene / LiCl mixed sol PGL; standing and degassing, molding, and placing in an oven for drying to form a film.
[0010] On the other hand, the method for preparing the moisture power generation gel material of the present invention comprises the following steps:
[0011] (1) Pour PVA into a solvent, heat and stir until the PVA is completely dissolved and becomes transparent, thereby obtaining a colorless and transparent PVA sol, wherein the mass ratio of PVA to solvent is 10 g:87.5-88.5 g;
[0012] (2) After the PVA sol is cooled to room temperature, the single-layer graphene is added to the PVA sol obtained in step (1), and heated and stirred until uniformly dispersed to obtain a PVA / single-layer graphene mixed sol PG, wherein the mass percentage of the single-layer graphene to the PVA is 0.5% to 1.5%;
[0013] (3) After the PG sol is cooled to room temperature, LiCl is added to the PG sol obtained in step (2), and heated and stirred until uniformly dispersed to obtain a PVA / single-layer graphene / LiCl mixed sol PGL, wherein the mass percentage of LiCl to PVA is 15% to 25%;
[0014] (4) The PGL sol obtained in step (3) is allowed to stand for degassing, and then the PGL sol is poured into a mold for molding, and placed in an oven for drying to form a film, thereby obtaining a moisture power generation gel material.
[0015] Preferably, in step (1), the solvent is deionized water.
[0016] Preferably, in step (1), the dissolution conditions of PVA are: stirring at 90-95° C. and 100-500 rpm for 2-3 hours until the PVA is completely dissolved and becomes transparent.
[0017] Most preferably, in step (1), the mass percentage of the single-layer graphene to the PVA is 1%;
[0018] Preferably, in step (2), the uniform dispersion conditions are: stirring at 85-95° C. and 100-500 rpm for 0.5-1.5 h to obtain sol PG.
[0019] Preferably, in step (3), the uniform dispersion conditions are: stirring at 90-95° C. and 100-500 rpm for 0.5-1.5 h to obtain the sol PGL.
[0020] Preferably, in step (4), the conditions for molding the sol PGL are: pouring the sol PGL into a rectangular mold with a length of 2 cm, a width of 2 cm, and a height of 1 cm, setting the drying temperature to 65-75° C., and the drying time to 6-8 h.
[0021] In another aspect, the wet gas power generation gel material of the present invention or the wet gas power generation gel material obtained by the above preparation method is used in the preparation of devices. The devices include breathing monitoring, humidity monitoring and flexible self-powered devices.
[0022] Beneficial effects: (1) The wet gas power generation gel material provided by the present invention is a blend of polymer PVA, single-layer graphene and LiCl, and its preparation method is simple and flexible, and can be applied to other wet gas power generation systems; (2) The wet gas power generation gel material provided by the present invention has good performance, is non-toxic, and can exist and operate stably; (3) The wet gas power generation gel material provided by the present invention fully combines the conductivity of single-layer graphene and the hygroscopicity of LiCl, and can generate electricity in a wide humidity range of 40% to 98% relative humidity, and the maximum average power generation voltage of a single block can reach 0.632V; (4) The wet gas power generation gel material provided by the present invention can respond to changes in environmental humidity, and has great application prospects in humidity monitoring, breathing monitoring, flexible self-power supply and other devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The figures are comparison diagrams of wet gas power generation performance output of PGL gel materials with different mass ratios prepared in Examples 1-3 under different humidity environments, wherein (a)-(c) are wet gas power generation behavior diagrams of mass ratios PVA:LiCl = 10:1; 5:1; 2:1 under relative humidity environments of 60% and 98%, respectively; (d)-(e) are morphological diagrams of the gel materials with corresponding mass ratios after completing the wet gas power generation test. DETAILED DESCRIPTION
[0024] Example 1: Preparation of wet gas power generation gel material
[0025] This embodiment provides a method for preparing a moisture power generation gel material, which specifically includes the following steps:
[0026] (1) Preparation of PVA sol: 10 g of polyvinyl alcohol (PVA, 1799 type) particles were placed in a 150 mL round-bottom flask, 88 g of deionized water was poured into the round-bottom flask, and the mixture was heated to 95 °C in an oil bath and stirred at 300 rpm for 2.5 h until the PVA was completely dissolved and became transparent, thereby obtaining a PVA sol;
[0027] (2) Preparation of PG sol: Remove the round-bottom flask, wait for the PVA sol to cool to room temperature (24°C), add 0.1 g of single-layer graphene to the round-bottom flask, heat to 95°C in an oil bath, and stir at 300 rpm for 1 h until the single-layer graphene is evenly dispersed to obtain a black PVA / single-layer graphene mixed PG sol;
[0028] (3) Preparation of 20% PGL sol by mass: Remove the round-bottom flask, wait for the PG sol to cool to room temperature (24°C), add 2 g LiCl to the round-bottom flask, heat to 95°C in an oil bath, and stir at 300 rpm for 1 h until the LiCl is evenly dispersed to obtain a black PVA / single-layer graphene / LiCl mixed PGL sol;
[0029] (4) Solidification and film formation: The round-bottom flask was removed, cooled to room temperature (24°C), and allowed to stand for degassing. The PGL sol was then poured into a rectangular mold with a length of 2 cm, a width of 2 cm, and a height of 1 cm. The mold was placed in an oven and the drying temperature was set to 70°C for 7 hours. After drying, a PGL gel material with wet gas power generation performance was obtained.
[0030] In the wet gas power generation gel material PGL film prepared in this example, the mass percentage of the single-layer graphene to PVA is 1%, and the mass percentage of LiCl to PVA is 20%.
[0031] The wet gas power generation performance was tested (the electrochemical workstation selected for the test experiment was CHI-760E model, the mode was set to open circuit voltage mode, the acquisition interval was set to 0.3s for one acquisition, and the total acquisition time was set to 600s). The specific test process is as follows: take a piece of PGL gel material, partially cover the top of the PGL material with copper tape, and the exposed PGL gel material is used as the moisture-sensitive part; use Al electrode to completely cover the bottom of the PGL to prevent the bottom from contacting the air. Connect the Cu electrode to the working electrode of the electrochemical workstation, and the Al electrode to the counter electrode of the electrochemical workstation to form a complete circuit. The electrochemical workstation can collect the voltage signal of the PGL gel material.
[0032] The relative humidity environment is constructed by using a saturated solution without inorganic salts. NaBr and K2SO4 saturated solutions were prepared in the experiment, and the relative humidity was 60% and 98% respectively. The PGL was placed in different relative humidity environments, and the difference in output voltage under different relative humidity was compared and analyzed.
[0033] The results are as follows: As shown in the figure, the average power generation voltage of 20% PGL gel material by mass in an environment with a relative humidity of 60% is 0.207V, and in an environment with a relative humidity of 98%, the average power generation voltage is 0.632V. It can be seen that the average power generation voltage of 20% PGL gel material is positively correlated with the relative humidity of the environment. The higher the relative humidity of the environment, the greater the average power generation. This shows that the 20% PGL gel material is humidity-sensitive and can reflect the relative humidity environment through power generation. This is the basis for PGL gel material to be applied to humidity detection and respiratory monitoring. At the same time, PGL gel has stable power generation, and there is no obvious attenuation of power generation voltage within 600s. During the power generation process, the morphology of the 20% PGL gel material remains stable, showing strong stability, which is the direct reason for ensuring stable power generation.
[0034] Example 2: Preparation of wet gas power generation gel material
[0035] This embodiment provides a method for preparing a moisture power generation gel material, which specifically includes the following steps:
[0036] (1) Preparation of PVA sol: 10 g of polyvinyl alcohol (PVA, 1799 type) particles were placed in a 150 mL round-bottom flask, 89 g of deionized water was poured into the round-bottom flask, and the mixture was heated to 95 °C in an oil bath and stirred at 300 rpm for 2.5 h until the PVA was completely dissolved and became transparent, thereby obtaining a PVA sol;
[0037] (2) Preparation of PG sol: Remove the round-bottom flask, wait for the PVA sol to cool to room temperature (24°C), add 0.1 g of single-layer graphene to the round-bottom flask, heat to 95°C in an oil bath, and stir at 300 rpm for 1 h until the single-layer graphene is evenly dispersed to obtain a black PVA / single-layer graphene mixed PG sol;
[0038] (3) Preparation of 20% PGL sol by mass: Remove the round-bottom flask, wait for the PG sol to cool to room temperature (24°C), add 1 g of LiCl to the round-bottom flask, heat the oil bath to 95°C, and stir at 300 rpm for 1 h until the LiCl is evenly dispersed to obtain a black PVA / single-layer graphene / LiCl mixed PGL sol;
[0039] (4) Solidification and film formation: The round-bottom flask was removed, cooled to room temperature (24°C), and allowed to stand for degassing. The PGL sol was then poured into a rectangular mold with a length of 2 cm, a width of 2 cm, and a height of 1 cm. The mold was placed in an oven and the drying temperature was set to 70°C for 7 hours. After drying, a PGL gel material with wet gas power generation performance was obtained.
[0040] In the wet gas power generation gel material PGL film prepared in this embodiment, the mass percentage of the single-layer graphene to PVA is 1%, and the mass percentage of LiCl to PVA is 10%.
[0041] The wet power generation test is the same as in Example 1, and the results are as follows: As shown in the figure, the average power generation voltage of the 10% mass ratio PGL gel material in an environment with a relative humidity of 60% is 0.185V, and in an environment with a relative humidity of 98%, the average power generation voltage is 0.239V. It can be seen that the average power generation of the 10% PGL gel material is also positively correlated with the relative humidity of the environment. Unlike Example 1, the average output voltage of the 10% PGL gel material is low and cannot reflect the characteristics of humidity sensitivity, so it cannot be used in humidity monitoring and respiratory monitoring. Similar to Example 1, the 10% PGL gel material can output a stable voltage, and the morphology can also be maintained as the initial membrane morphology, so no obvious output voltage decay phenomenon was observed within 600s.
[0042] Example 3: Preparation of wet gas power generation gel material
[0043] (1) Preparation of PVA sol: 10 g of polyvinyl alcohol (PVA, 1799 type) particles were placed in a 150 mL round-bottom flask, 85 g of deionized water was poured into the round-bottom flask, and the mixture was heated to 95 °C in an oil bath, and stirred at 300 rpm for 2.5 h until the PVA was completely dissolved and became transparent, thereby obtaining a PVA sol;
[0044] (2) Preparation of PG sol: Remove the round-bottom flask, wait for the PVA sol to cool to room temperature (24°C), add 0.1 g of single-layer graphene to the round-bottom flask, heat to 95°C in an oil bath, and stir at 300 rpm for 1 h until the single-layer graphene is evenly dispersed to obtain a black PVA / single-layer graphene mixed PG sol;
[0045] (3) Preparation of 20% by mass PGL sol: Remove the round-bottom flask, wait for the PG sol to cool to room temperature (24°C), add 5 g of LiCl to the round-bottom flask, heat the oil bath to 95°C, and stir at 300 rpm for 1 h until the LiCl is evenly dispersed to obtain a black PVA / single-layer graphene / LiCl mixed PGL sol;
[0046] (4) Solidification and film formation: The round-bottom flask was removed, cooled to room temperature (24°C), and allowed to stand for degassing. The PGL sol was then poured into a rectangular mold with a length of 2 cm, a width of 2 cm, and a height of 1 cm. The mold was placed in an oven and the drying temperature was set to 70°C for 7 hours. After drying, a PGL gel material with wet gas power generation performance was obtained.
[0047] In the wet gas power generation gel material PGL film prepared in this embodiment, the mass percentage of the single-layer graphene to PVA is 1%, and the mass percentage of LiCl to PVA is 50%.
[0048] The wet gas power generation test is the same as that in Example 1, and the results are as follows: as shown in the figure, for a 50% mass ratio PGL gel material, in an environment with a relative humidity of 60%, the average power generation voltage is 0.57V, and in an environment with a relative humidity of 98%, the average power generation voltage is 0.60V. It can be seen that the average power generation of the 50% PGL gel material also shows a weak positive correlation with the relative humidity of the environment; different from Example 1, in an environment with a relative humidity of 60%, the average output voltage of the 50% PGL gel material is greater than that of the 20% PGL gel material, but in an environment with a relative humidity of 98%, the average output voltage of the 50% PGL gel material is less than that of the 20% PGL gel material. It can be seen that the 50% PGL gel material can maintain a relatively high voltage output at a relative humidity of 60%-98%, but its maximum average voltage output is weaker than that of the 20% PGL gel material; at the same time, different from Example 1, after the wet gas power generation test of the 50% PGL gel material is completed, it is difficult for the film to maintain its initial shape, which is the direct reason for the large fluctuation in the voltage output of the 50% PGL gel material.
[0049] According to the results of Examples 1-3, a PGL gel material with a LiCl to PVA mass ratio of 20% was selected for wet gas power generation, which has the best electrical output performance and can ensure stability during operation, while being able to respond to different humidity environments.
[0050] Example 4: Preparation of wet gas power generation gel material
[0051] The difference between this embodiment and embodiment 1 is that the amount of single-layer graphene added is different. In step (2), 0.05g single-layer graphene and 0.15g single-layer graphene are used to replace 0.1g single-layer graphene respectively to prepare the wet gas power generation gel material. The remaining preparation steps are the same as those in embodiment 1. The wet gas power generation gel material finally prepared can respond to the humidity environment.
[0052] Example 5: Preparation of wet gas power generation gel material
[0053] The difference between this embodiment and embodiment 1 is that the amount of LiCl added is different. In step (3), 1.5g LiCl and 2.5g LiCl are used to replace 2g LiCl respectively to prepare the wet gas power generation gel material. The remaining preparation steps are the same as those in embodiment 1. The wet gas power generation gel material finally prepared can respond to the humidity environment.
[0054] The moisture power generation gel material provided by the present invention fully combines the conductivity of single-layer graphene and the hygroscopicity of LiCl, and can generate electricity in a wide humidity range of 40% to 98% relative humidity. The maximum average power generation voltage of a single block can reach 0.632V.
Claims
1. A moisture power generation gel material, It is characterized in that The gel material comprises PVA, single-layer graphene and LiCl, the mass percentage of the single-layer graphene to PVA is 0.5% to 1.5%, and the mass percentage of the LiCl to PVA is 10% to 50%.
2. The moisture power generation gel material according to claim 1, It is characterized in that The mass percentage of the single-layer graphene to PVA is 1%, and the mass percentage of LiCl to PVA is 15%-25%.
3. The moisture power generation gel material according to claim 1, It is characterized in that The PVA is PVA 1799 type.
4. A method for preparing a moisture power generation gel material according to any one of claims 1 to 3, It is characterized in that The following steps are involved: (1) Pour PVA into a solvent, heat and stir until the PVA is completely dissolved and becomes transparent, thereby obtaining a colorless and transparent PVA sol; (2) After the PVA sol is cooled to room temperature, the single-layer graphene is added to the PVA sol obtained in step (1), and heated and stirred until uniformly dispersed to obtain a PVA / single-layer graphene mixed sol PG; (3) After the PG sol is cooled to room temperature, LiCl is added to the PG sol obtained in step (2), and heated and stirred until uniformly dispersed to obtain a PVA / single-layer graphene / LiCl mixed sol PGL; (4) The PGL sol obtained in step (3) is allowed to stand for degassing, and then the PGL sol is poured into a mold for molding, and dried to form a film, thereby obtaining a wet gas power generation gel material.
5. The preparation method according to claim 5, It is characterized in that In step (1), the solvent is deionized water.
6. The preparation method according to claim 5, It is characterized in that In step (1), the dissolution conditions of PVA are: stirring at 90-95° C. and 100-500 rpm for 2-3 hours until the PVA is completely dissolved and becomes transparent.
7. The preparation method according to claim 5, It is characterized in that In step (2), the uniform dispersion conditions are: stirring at 85-95° C. and 100-500 rpm for 0.5-1.5 h to obtain sol PG.
8. The preparation method according to claim 5, It is characterized in that In step (3), the uniform dispersion conditions are: stirring at 90-95° C. and 100-500 rpm for 0.5-1.5 h to obtain the sol PGL.
9. The preparation method according to claim 5, It is characterized in that In step (4), the conditions for forming the sol PGL are as follows: pouring the sol PGL into a mold, setting the drying temperature to 65-75° C., and drying time to 6-8 h.
10. Use of the moisture power generation gel material according to any one of claims 1 to 3 in the preparation of respiratory monitoring devices.