ASA material with uniform light effect and preparation method thereof

Through the multi-component composite and twin-screw extruder blending process, the composition and process of ASA materials are optimized, and the problems of poor transmittance and poor uniform light effect of ASA materials are solved, achieving high transmittance and high fog The uniform light effect of degree and maintains impact resistance, suitable for automotive parts and exterior parts.

CN119081331APending Publication Date: 2024-12-06ZHEJIANG KEPUTE NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411451868.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-17
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Due to the difference in glass transition temperature of the rubber phase, ASA materials have poor light transmittance, which affects their use in areas with high optical performance requirements.

Method used

ASA materials are prepared by multi-component composite through twin-screw extruder blending, including AS resin, ASA glue powder, PMMA resin, TPU elastomer, polysiloxane and processing aids, optimize their mass ratio and melting. Mixed process to achieve uniform light visual effect.

Benefits of technology

It improves the light transmittance of ASA materials by more than 50% and haze by more than 90%, meets optical requirements and maintains impact resistance, simplifies process flow and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081331A_ABST
    Figure CN119081331A_ABST
Patent Text Reader

Abstract

The invention discloses an ASA material with a light uniformizing effect and a preparation method thereof, and the ASA material with the light uniformizing effect is obtained by melting and mixing AS resin, ASA rubber powder, PMMA resin, TPU elastomer, polysiloxane and a processing aid. For plastic parts, especially non-paint-spraying plastic parts, comprehensive improvement of mechanical properties and optical properties (light uniformizing performance) is difficult to achieve, the ASA material replacing ABS as the non-paint-spraying plastic parts in the market at present does not have the light uniformizing effect, and the ASA material with the light uniformizing effect obtained by the invention has the advantages that the light uniformizing effect is achieved; the problems that an existing ASA material replacing ABS to serve as a main material of non-paint-spraying plastic parts is poor in light transmittance and light uniformizing effect are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to new material technology, and specifically relates to an ASA material with a uniform light effect and a preparation method thereof. Background Art

[0002] ASA materials have stronger weather resistance than ABS because the main chains of the molecular chains are all saturated carbon chains. They are widely used in outdoor products and automotive exterior parts, replacing ABS as one of the main materials for non-painted plastic parts. Compared with ABS, the rubber of ASA is replaced by acrylic rubber instead of butadiene. Due to the difference in glass transition temperature of the rubber segment, ASA usually needs to increase the particle size of the rubber phase (compared with the rubber phase in ABS materials) to obtain better impact toughness, which results in poor light transmittance of ASA materials (compared with ABS materials), affecting the use of ASA materials in some fields with high requirements for optical properties. Summary of the invention

[0003] The present invention adopts the synergistic effect of different polymers to affect the propagation of light, and prepares the ASA material with uniform light visual effect by multi-component compounding and blending in a twin-screw extruder.

[0004] The present invention adopts the following technical scheme.

[0005] An ASA material with a uniform light effect comprises AS resin, ASA rubber powder, PMMA resin, TPU elastomer, polysiloxane and a processing aid.

[0006] In the present invention, the mass ratio of AS resin, ASA rubber powder, PMMA resin, TPU elastomer, polysiloxane and processing aid is (20-40): (20-40): (25-40): (5-20): (2-5): (1-3); preferably, the mass ratio of AS resin, ASA rubber powder, PMMA resin, TPU elastomer, polysiloxane and processing aid is (20-30): (25-35): (30-40): (5-15): (2-4): (1-3).

[0007] In the present invention, AS resin is a polystyrene-acrylonitrile copolymer with a melt index of 5 to 30 g / 10 min (220° C., 10 kg condition); in the ASA rubber powder, the rubber content is 50% to 60% and the particle size is 200 nm to 300 nm; the melt index of PMMA resin is 1 to 3 g / 10 min (230° C., 3.8 kg condition); and the TPU elastomer is aliphatic PCL type with a hardness of 70A to 90A.

[0008] In the present invention, the polysiloxane is silicone powder; the processing aids include antioxidants, anti-UV agents and lubricants.

[0009] The invention discloses a method for preparing the ASA material with the above-mentioned light-homogenizing effect, comprising the following steps: melt-mixing AS resin, ASA rubber powder, PMMA resin, TPU elastomer, polysiloxane and processing aid to obtain the ASA material with the light-homogenizing effect.

[0010] Preferably, the melt mixing is carried out in a screw extruder, and the specific screw extruder and extrusion parameters are conventional technologies.

[0011] The present invention discloses the use of the ASA material with the above light-homogenizing effect in the preparation of a light-homogenizing material. Preferably, the light-homogenizing material has a transmittance greater than 50% and a haze greater than 90%.

[0012] The invention discloses the application of the ASA material with the light-homogenizing effect in the preparation of automobile materials, especially in the preparation of automobile non-painting plastics.

[0013] Therefore, the present invention discloses an outdoor product or an automobile component exterior trim, which is prepared from the ASA material with the above-mentioned light-homogenizing effect.

[0014] There are two main types of ASA materials that can replace ABS as non-painted plastic parts on the market. One type has low light transmittance, usually less than 20% (sample thickness 3.2mm), haze of more than 90%, and greater light blocking; the other type of ASA alloy material has a light transmittance of up to 40%, but haze of less than 50%, slightly greater light blocking and insufficient light-distribution effect (partially visible font information under the sample). The present invention can achieve a visual effect of light distribution, meet optical requirements and key impact resistance requirements; and the process is simple, efficient and low cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 The figures are actual photos of different ASA materials, 1# is comparison group 4, 2# is the existing commercially available product, 3# is example 2, 4# is example 3, and 5# is example 1. DETAILED DESCRIPTION

[0016] The invention uses AS resin, ASA rubber powder, PMMA resin, TPU elastomer, polysiloxane and processing aid as raw materials, melts and mixes them, and obtains ASA material with uniform light effect, thereby solving the problem that the existing ASA material which replaces ABS as the main material of non-painted plastic parts has poor light transmittance and poor uniform light effect.

[0017] According to mass percentage, the formula of raw materials of the present invention (total 100%) is as follows: AS resin balance ASA rubber powder 20-40% PMMA resin 25-40% TPU elastomer 5-20% Polysiloxane 2-5% Processing aids 1-3%.

[0018] in: AS resin: polystyrene-acrylonitrile copolymer, melt index is 5-30g / 10min (220℃, 10kg condition), preferably melt index is 8-15g / 10min (220℃, 10kg condition); ASA rubber powder: rubber content 50%-60%, particle size 200nm-300nm; PMMA resin: melt index 2g / 10min (230℃, 3.8kg condition); TPU resin: aliphatic PCL type, hardness 70A-90A; Polysiloxane: silicone powder; Processing aids: antioxidants, anti-UV agents and lubricants.

[0019] The invention discloses a processing method of an ASA material with a uniform light effect: the raw materials are pre-mixed and then directly put into a twin-screw extruder for melting and mixing to form particles; the twin-screw equipment used has a diameter of 30-75 mm, a rotation speed of 300-1200 rpm, a temperature of 200-250° C., and is processed into particles.

[0020] Material testing methods: Flexural modulus: According to ISO 178, rate 2mm / min, required to be above 2000MPa; Impact strength: According to ISO 179-1eA, room temperature, requirement 13kj / m 2 above; Transmittance and haze: According to ASTM D1003, the thickness of the test piece is 3.2mm, and the transmittance is required to be no less than 50% and the haze is required to be no less than 90%; Melt index: According to ISO 1133, condition 220℃, 10kg, requirement is 5g / 10min or more.

[0021] The following is an explanation of the technical progress of the present invention through specific experiments. The raw materials used are all existing products, and the specific preparation operations and performance tests are all conventional techniques. Example

[0022] AS resin is PN-138H; ASA rubber powder is BS-006 from Ningbo Benshuo Technology; PMMA resin: Suzhou Shuangxiang SX-304; TPU resin: Meirui New Materials A885; polysiloxane: silicone powder, Shaoxing Jiahua SG600; SEBS-g-MAH: Kraton FG1901; processing aids: antioxidants, anti-UV agents and lubricants, among which antioxidants are 1010 and 168, each accounting for 0.2%, anti-UV agents are 770 and 234, each accounting for 0.3%, and lubricant is PETS, accounting for 1%.

[0023] Table 1 Examples and Comparative Examples Formula, Kg

[0024] Processing method of ASA material: According to Table 1, the raw materials are pre-mixed in a high-speed mixer and then directly extruded into a twin-screw extruder for melting and mixing to form particles; the twin-screw equipment used has a diameter of 50 mm, a rotation speed of 800 rpm, and a temperature of 200-250°C (200°C, 205°C, 210°C, 215°C, 220°C, 225°C, 230°C, 235°C, 240°C, 250°C), and the materials are processed into particles.

[0025] The material performance test results are shown in Table 2. AS resin, ASA rubber powder, PMMA resin, TPU elastomer, polysiloxane and processing aids are used as raw materials and melt mixed to obtain ASA materials with uniform light effect, which meet the application requirements of automotive exterior parts. In contrast, ASA materials or ASA alloys cannot achieve comprehensive improvement in mechanical and optical properties. Both PMMA blending and SEBS modification have defects in uniform light performance and mechanical properties, resulting in unqualified products. Although the SEBS modified group improves the impact strength, the flexural modulus is significantly reduced to less than 1900MPa.

[0026] Table 2 Properties of ASA materials prepared in Examples and Comparative Examples

[0027] For plastic parts, especially unpainted plastic parts, it is difficult to achieve a comprehensive improvement in mechanical properties and optical properties (light-distribution performance). Currently, there are two main types of ASA materials on the market that can replace ABS as unpainted plastic parts. One type has low light transmittance, usually less than 20%, and a haze of more than 90%, which blocks light more; the other type of ASA alloy material has a light transmittance of up to 45%, but a haze of less than 50%, which blocks light slightly and has insufficient light-distribution effect, which can be partially seen in the font information below the sample, see Figure 1ASA material has poor light transmittance, but high haze and good mechanical properties (flexural modulus up to 2382MPa, compared with group 1); the more PMMA is added, the greater the light transmittance, but the haze decreases significantly, and the impact strength also decreases; SEBS-g-MAH can improve light transmittance, but the haze is low and MAH is slightly yellowish, which is not conducive to its application as unpainted plastic parts, see Figure 1 1#, especially the mechanical properties decreased significantly.

[0028] Comparative Example 8 On the basis of Example 1, 3 kg of polysiloxane was replaced by an equal amount of AS resin, that is, polysiloxane was omitted and 28 kg of AS resin was used. The rest was the same, and the processing and granulation were carried out. The haze of the test sample was 82%.

[0029] On the basis of Example 1, 10 kg of TPU elastomer was replaced by an equal amount of AS resin, that is, TPU elastomer was omitted and 35 kg of AS resin was used. The rest was the same, and the processing and granulation were carried out. The transmittance of the test sample was 45%.

[0030] The modification of TPU alone reduces the haze, and the modification of silicone alone reduces the light transmittance. The present invention uses AS resin, ASA rubber powder, PMMA resin, TPU elastomer, polysiloxane, and processing aid as raw materials, and melts and mixes them to obtain an ASA material with a uniform light effect. Not only is the light transmittance greater than 50%, the haze is greater than 90%, and the uniform light effect is achieved. Figure 1 3#~5#, and basically maintain the mechanical properties of ASA material (flexural modulus above 2300MPa, impact strength 14kj / m 2 above).

Claims

1. An ASA material with a uniform light effect, comprising AS resin, ASA rubber powder, PMMA resin, TPU elastomer, polysiloxane, and processing aid.

2. The ASA material with light-homogenizing effect according to claim 1, characterized in that: The mass ratio of AS resin, ASA rubber powder, PMMA resin, TPU elastomer, polysiloxane and processing aid is (20-40): (20-40): (25-40): (5-20): (2-5): (1-3).

3. The ASA material with light-homogenizing effect according to claim 2, characterized in that: The mass ratio of AS resin, ASA rubber powder, PMMA resin, TPU elastomer, polysiloxane and processing aid is (20-30): (25-35): (30-40): (5-15): (2-4): (1-3).

4. The ASA material with light-homogenizing effect according to claim 1, characterized in that: The melt index of AS resin is 5-30g / 10min; the rubber content of ASA rubber powder is 50%-60%, and the particle size is 200nm-300nm; the melt index of PMMA resin is 1-3g / 10min; the hardness of TPU elastomer is 70A-90A.

5. The ASA material with light-homogenizing effect according to claim 1, characterized in that: The polysiloxane is silicone powder; the processing aids include antioxidants, anti-UV agents, and lubricants.

6. The method for preparing the ASA material with uniform light effect according to claim 1, characterized in that: The method comprises the following steps: melting and mixing AS resin, ASA rubber powder, PMMA resin, TPU elastomer, polysiloxane and processing aid to obtain ASA material with uniform light effect.

7. The method for preparing the ASA material with uniform light effect according to claim 6, characterized in that: Melt mixing is carried out in a screw extruder.

8. Use of the ASA material with light-homogenizing effect as claimed in claim 1 in the preparation of light-homogenizing materials.

9. Use of the ASA material with light-homogenizing effect as claimed in claim 1 in the preparation of automotive materials.

10. An outdoor product or automobile component exterior trim, prepared from the ASA material with light-homogenizing effect as claimed in claim 1.