Antistatic ABS reclaimed material and preparation method thereof

By using polydopamine chemically grafted carbon nanotubes and organic antistatic agents in ABS recycled materials, combining diphenylmethane diisooxylate and coupling agent, the deficiency of antistatic properties in the prior art and The high cost problem has achieved efficient anti-static and mechanical performance improvements, meeting the needs of high standards and long-term anti-static.

CN119081339APending Publication Date: 2024-12-06DONGGUAN YUJIE IND INVESTMENT CO LTD

Patent Information

Application Number
CN202411249784.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing antistatic ABS recycled materials are prone to static electricity in dry environments and cannot meet the needs of high standards and long-term antistatic electricity. The commonly used carbon nanotube conductive fillers increase material cost and mechanical performance losses.

Method used

The combination of polydopamine chemical grafted carbon nanotubes and organic antistatic agents is used as composite antistatic agents. Through reasonable proportions and process conditions, the compatibility and dispersion of materials are improved, and diphenylmethane diisooxygen is combined Acid esters and coupling agents improve antistatic and mechanical properties.

Benefits of technology

The excellent antistatic properties and mechanical properties of antistatic ABS recycled materials have been achieved, the amount of antistatic agent is used, the impact strength and tensile performance are improved, and the high standard and long-term antistatic requirements are met, while the production costs and Dust pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005031922870000091
    Figure BDA0005031922870000091
Patent Text Reader

Abstract

The invention relates to the field of antistatic materials, in particular to an antistatic ABS reclaimed material and a preparation method thereof. The invention relates to an antistatic ABS (Acrylonitrile Butadiene Styrene) regenerated material, which is prepared from the following raw materials in parts by mass: 90 to 95 parts of ABS regenerated material, 5 to 7 parts of composite antistatic agent, 4 to 5 parts of diphenylmethane diisooxyl ester, 2 to 3 parts of coupling agent and 0.3 to 0.4 part of antioxidant. The antistatic ABS reclaimed material provided by the invention has excellent antistatic performance and mechanical properties, and can meet application scenarios with high-standard and long-time antistatic requirements. By introducing the diphenylmethane diisoxo acid ester and the composite antistatic agent, the viscosity and molecular weight of the antistatic ABS reclaimed material are improved, broken chains in the ABS reclaimed material are repaired, the mechanical property is improved, and particularly, the tensile property is remarkably improved. Meanwhile, the compound of the polydopamine chemically grafted carbon nanotubes and the organic antistatic agent is adopted as the composite antistatic agent, so that the dosage of the antistatic agent is reduced, the compatibility and dispersity of the composite antistatic agent and the ABS regenerated material are improved, and the mechanical property and antistatic efficiency of the antistatic ABS regenerated material are further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of antistatic materials, and in particular to an antistatic ABS recycled material and a preparation method thereof. Background Art

[0002] As a common polymer material, ABS resin is widely used in electronics, automobiles, home appliances and other fields. With the increasing attention paid to resource recycling, the research and application of ABS recycled materials are becoming more and more active. However, ordinary ABS recycled materials are prone to static electricity in a dry environment, which brings safety hazards to use.

[0003] In the prior art, carbon nanotubes are usually used as conductive fillers to improve the antistatic properties of ABS resin, which cannot meet the application scenarios with high standards and long-term antistatic requirements. For example, the Chinese patent application with application number CN102268171A discloses a new antistatic resin material and its preparation method. The invention utilizes the synergistic effect between carbon black, carbon nanotubes and polyaniline, and prepares ABS composite materials by directly blending them, so that the material meets the antistatic requirements. However, due to the high content of added carbon black, the mechanical properties of the material are greatly lost. The Chinese patent application with application number CN110615953A discloses an antistatic ABS composite material and its preparation method. The invention introduces ionic liquid as a compatibilizer for ABS resin and carbon nanotubes. By adding 2-5 parts of carbon nanotube antistatic agent, the surface resistance of the material reaches 10 5 Ω, but the price of ionic liquids is relatively expensive, which increases the cost of material preparation. Summary of the invention

[0004] The purpose of this application is to provide an antistatic ABS recycled material and a preparation method thereof in response to the deficiencies of current technology. The antistatic ABS recycled material prepared in this application has excellent antistatic properties and mechanical properties, and can meet application scenarios with high standards and long-term antistatic requirements.

[0005] In the first aspect, the present application provides an antistatic ABS recycled material, which adopts the following technical solution: An antistatic ABS recycled material comprises the following raw materials by weight: 90-95 parts of ABS recycled material, 5-7 parts of composite antistatic agent, 4-5 parts of diphenylmethane diisocyanate, 2-3 parts of coupling agent and 0.3-0.4 parts of antioxidant.

[0006] By adopting the above technical scheme, the antistatic ABS recycled material of the present application has excellent antistatic properties and mechanical properties, and can meet the application scenarios with high standards and long-term antistatic requirements. ABS recycled material: As the main raw material, it provides basic physical and chemical properties. Composite antistatic agent: The compounding of polydopamine chemically grafted carbon nanotubes and organic antistatic agents significantly reduces the amount of antistatic agent used, while improving the compatibility and dispersibility of the composite antistatic agent with ABS recycled materials, thereby improving the mechanical properties (such as impact strength) and antistatic efficiency of the antistatic ABS recycled materials. Diphenylmethane diisocyanate: After its introduction, it leads to the entanglement of molecular chains, increases the viscosity and molecular weight of antistatic ABS recycled materials, repairs the broken chains in ABS recycled materials, and improves the mechanical properties, especially the tensile properties. It is significantly improved. Coupling agent: Improves the interfacial adhesion of the composite material and improves the mechanical properties of the material. Antioxidant: Prevents the oxidative degradation of the material during processing and use, and extends the service life of the material. The above components work synergistically through reasonable proportions and process conditions, so that the antistatic ABS recycled material of the present application has excellent antistatic properties and mechanical properties.

[0007] Preferably, the ABS recycled material is recovered by a recycling method, and the recycling method comprises the following steps: S21, coarsely crushing the recovered ABS recycled material to obtain ABS recycled material fragments with a particle size of ≤30 mm; S22, performing preliminary cleaning on the ABS recycled material fragments, including pickling, rinsing and drying in sequence; S23, freezing the ABS recycled material after preliminary cleaning for 10-30 minutes, with the freezing temperature being -40°C to -20°C; S24 finely grinds the frozen ABS recycled material to a particle size of 1-4 mm; washes the finely grinded ABS recycled material with a sodium chloride solution with a mass concentration of 5.5-6.5 g / L, rinses it after washing, and then dries it at 60-70° C. for 20-36 hours to obtain ABS recycled material.

[0008] By adopting the above technical scheme, the ABS recycled material of the present application is obtained by a specific recycling method, which includes the steps of coarse crushing, preliminary cleaning, freezing treatment, fine crushing and sodium chloride solution cleaning. Coarse crushing: The recovered ABS recycled material is coarsely crushed to obtain ABS recycled material fragments with a particle size of ≤30mm. This step helps to reduce the volume of the material and facilitate subsequent processing. Preliminary cleaning: The ABS recycled material fragments are preliminarily cleaned, including acid washing, rinsing and drying in sequence. This step can remove impurities and contaminants on the surface and improve the quality of the ABS recycled material. Freezing treatment: The ABS recycled material after preliminary cleaning is frozen for 10-30 minutes, and the freezing temperature is -40℃ to -20℃. This step can freeze the moisture in the ABS recycled material, which is convenient for the subsequent fine crushing process. Fine crushing: The frozen ABS recycled material is finely crushed to a particle size of 1-4mm. This step can further reduce the particle size of the material and improve the performance of the ABS recycled material. Sodium chloride solution cleaning: The finely crushed ABS recycled material is cleaned with a sodium chloride solution with a mass concentration of 5.5-6.5g / L, rinsed after cleaning, and then dried at 60-70℃ for 20-36h to obtain ABS recycled material. This step can remove residual impurities and pollutants and improve the quality of ABS recycled material. Through the synergistic effect of the above steps, high-quality ABS recycled material can be obtained to meet the application scenarios with high standards and long-term antistatic requirements. At the same time, this method reduces dust pollution, fragment loss and crushing efficiency during the crushing process, which is more environmentally friendly and convenient.

[0009] Preferably, the composite antistatic agent is prepared by mixing polydopamine chemically grafted carbon nanotubes and an organic antistatic agent in a mass ratio of 8:2-3.

[0010] By adopting the above technical scheme, through the compounding of polydopamine chemically grafted carbon nanotubes and organic antistatic agents, excellent antistatic performance can be achieved at a lower addition amount, thereby reducing the amount of antistatic agent used. The synergistic effect between polydopamine chemically grafted carbon nanotubes and organic antistatic agents improves the compatibility between the composite antistatic agent and ABS recycled materials, and at the same time improves the dispersibility of the antistatic agent in ABS recycled materials. The addition of the composite antistatic agent can improve the mechanical properties of the antistatic ABS recycled materials, such as impact strength. The synergistic effect of the composite antistatic agent improves the antistatic efficiency of the antistatic ABS recycled materials, thereby meeting the application scenarios with high standards and long-term antistatic requirements. Polydopamine chemically grafted carbon nanotubes have excellent conductive properties, can effectively conduct static charges, reduce the resistivity of the material surface, and thus improve the antistatic performance. The organic antistatic agent has good compatibility and dispersibility, can form a uniform mixture with ABS recycled materials, improve the uniformity of the distribution of the antistatic agent in the material, and thus improve the antistatic performance. The synergistic effect between polydopamine chemically grafted carbon nanotubes and organic antistatic agents can enable the composite antistatic agent to achieve excellent antistatic performance at a lower addition amount, reducing production costs. The synergistic effect between polydopamine chemically grafted carbon nanotubes and organic antistatic agents can also improve the mechanical properties of antistatic ABS recycled materials, thereby meeting a wider range of application needs.

[0011] Preferably, the method for preparing polydopamine chemically grafted carbon nanotubes comprises the following steps: S41, placing 10 parts of carbon nanotubes in a mixed acid consisting of 70 parts of nitric acid with a mass concentration of 65% and 30 parts of sulfuric acid with a mass concentration of 98%, ultrasonically treating for 8-10 hours, cooling, diluting with deionized water, and filtering, washing the filter cake with distilled water to obtain hydroxylated carbon nanotubes; S42, according to the mass fractions, add 30 parts of γ-aminopropyltriethoxysilane and 2.5-3 parts of distilled water into a container and mix them evenly at room temperature, stir them thoroughly at room temperature, then slowly heat up to 50-55° C., react for 5-8 hours to obtain a colorless transparent liquid, and vacuum dry to obtain amino-terminated hyperbranched polysiloxane; S43. According to the mass fractions, add polydopamine, amino-terminated hyperbranched polysiloxane and hydroxylated carbon nanotubes to isopropanol in sequence under stirring, stir and mix, and finally add ammonia water to adjust the pH of the system to 7-8, continue stirring for 2-3 hours, and then let it stand for 4-5 hours to obtain polydopamine chemically grafted carbon nanotubes.

[0012] By adopting the above technical scheme, the preparation method of polydopamine chemically grafted carbon nanotubes involves the following steps: S41, preparation of hydroxylated carbon nanotubes: First, a certain amount of carbon nanotubes are placed in a mixed acid composed of nitric acid and sulfuric acid, and dispersed and acid-activated by ultrasonic treatment. The ultrasonic treatment can last for 8-10 hours, and this process will introduce hydroxyl (-OH) functional groups on the surface of the carbon nanotubes. Subsequently, the mixture is cooled and diluted with deionized water, and then the solid is separated by suction filtration. After washing the filter cake, hydroxylated carbon nanotubes are obtained, and these hydroxyl functional groups are conducive to the subsequent reaction. S42, synthesis of amino-terminated hyperbranched polysiloxane: γ-aminopropyltriethoxysilane and a small amount of distilled water are mixed and stirred evenly at room temperature. After that, the temperature is slowly raised to 50-55°C and maintained for 5-8 hours to promote the reaction, and finally a colorless transparent liquid is obtained. After the liquid is vacuum dried, amino-terminated hyperbranched polysiloxane is obtained, which contains a highly reactive amino (-NH2) terminal group. S43, synthesis of polydopamine chemically grafted carbon nanotubes: polydopamine, amino-terminated hyperbranched polysiloxane, and previously prepared hydroxylated carbon nanotubes are sequentially added to an isopropanol solvent under stirring. After these components are uniformly mixed under stirring, ammonia water is added to adjust the pH value of the system to 7-8, and stirring is continued for 2-3 hours. Then, the mixture is allowed to stand for 4-5 hours to complete the grafting reaction between polydopamine and carbon nanotubes to form polydopamine chemically grafted carbon nanotubes.

[0013] After polydopamine is chemically grafted onto carbon nanotubes, the high conductivity of carbon nanotubes and the charge transfer characteristics of polydopamine can be used to effectively improve the antistatic properties of ABS recycled materials. Carbon nanotubes themselves have extremely high strength and modulus. After being grafted into ABS recycled materials, they can significantly improve the mechanical properties of the material, especially the tensile properties and impact strength. Improve compatibility and dispersibility: Endamine hyperbranched polysiloxane as a coupling agent helps to improve the dispersibility of carbon nanotubes in the ABS matrix, reduce agglomeration, and increase the interfacial interaction between carbon nanotubes and ABS, thereby improving the overall performance of the material. In summary, the introduction of polydopamine chemically grafted carbon nanotubes not only improves the antistatic properties, but also has a significant enhancement effect on the mechanical properties of the material, and its good compatibility and dispersibility with ABS recycled materials is the key to achieving this goal.

[0014] Preferably, in step S43, the mass ratio of the isopropanol, polydopamine, amino-terminated hyperbranched polysiloxane and hydroxylated carbon nanotubes is 60:17:26:(8-10).

[0015] Preferably, the organic antistatic agent is a block copolymer of nylon 6 and ethylene oxide.

[0016] Preferably, the coupling agent is composed of vinyltrichlorosilane, vinyltrimethoxysilane and γ-aminopropyltriethoxysilane in a mass ratio of 2:3:5.

[0017] By adopting the above technical scheme, the coupling agent is composed of vinyl trichlorosilane, vinyl trimethoxysilane and γ-aminopropyl triethoxysilane in a mass ratio of 2:3:5. These coupling agents play a key role in the preparation process of antistatic ABS recycled materials. They can improve the compatibility and dispersibility between the antistatic agent and the ABS recycled materials, thereby improving the mechanical properties (such as impact strength) and antistatic efficiency of the antistatic ABS recycled materials. Vinyl trichlorosilane, vinyl trimethoxysilane and γ-aminopropyl triethoxysilane work synergistically to tightly combine the antistatic agent with the ABS recycled materials through chemical bonding to form a stable composite material. This structure not only improves the dispersibility of the antistatic agent in the ABS recycled materials, but also enhances the interaction between the antistatic agent and the ABS recycled materials, thereby improving the overall performance of the antistatic ABS recycled materials. In addition, these coupling agents can also repair the broken chains in the ABS recycled materials and further improve their mechanical properties. In short, in this application, the synergistic effect of the coupling agent is of great significance for improving the performance of the antistatic ABS recycled materials.

[0018] Preferably, the antioxidant consists of antioxidant 1010 and antioxidant 1076 in a mass ratio of 3:1.

[0019] In the second aspect, the present application provides a method for preparing an antistatic ABS recycled material, using the following technical solution: As a general technical concept, the present application also provides a method for preparing the above-mentioned antistatic ABS recycled material, comprising the following steps: S91. Evenly mix the ABS recycled material, the composite antistatic agent, the diphenylmethane diisocyanate, the coupling agent and the antioxidant in a high-speed mixer according to their weight fractions to obtain a mixture; S92, feeding the mixed material into a twin-screw extruder through an automatic feeding system for melt extrusion and granulation to obtain antistatic ABS recycled material.

[0020] Preferably, the twin-screw extruder comprises a first zone, a second zone, a third zone, a fourth zone, a fifth zone and a sixth zone connected in sequence, wherein the temperature of the first zone is 170-180°C, the temperature of the second zone is 170-180°C, the temperature of the third zone is 180-190°C, the temperature of the fourth zone is 180-190°C, the temperature of the fifth zone is 180-190°C, and the temperature of the sixth zone is 180-190°C.

[0021] In summary, the beneficial technical effects of this application are: 1. Excellent antistatic performance: The use of composite antistatic agents significantly reduces the amount of antistatic agents used, while improving the antistatic efficiency. This makes the prepared antistatic ABS recycled material have excellent antistatic performance and can meet the application scenarios with high standards and long-term antistatic requirements.

[0022] 2. Good mechanical properties: The introduction of diphenylmethane diisocyanate leads to the entanglement of molecular chains, increases the viscosity and molecular weight of antistatic ABS recycled materials, repairs the broken chains in ABS recycled materials, thereby improving the mechanical properties, especially the tensile properties.

[0023] 3. Environmentally friendly and convenient recycling method: The recycling method of ABS recycled materials is to firstly crush the recycled ABS recycled materials, preliminarily clean them and freeze them at -40℃ to -20℃, and finally crush them to a particle size of 1-4mm and clean them with sodium chloride solution. This method greatly reduces dust pollution, chip loss and crushing efficiency during the crushing process, and is more environmentally friendly and convenient.

[0024] 4. Improve the mechanical properties and antistatic efficiency of antistatic ABS recycled materials: The composite antistatic agent adopts the compound of polydopamine chemically grafted carbon nanotubes and organic antistatic agent, which significantly reduces the amount of antistatic agent, and at the same time improves the compatibility and dispersibility of the composite antistatic agent with ABS recycled materials, thereby improving the mechanical properties (such as impact strength) and antistatic efficiency of antistatic ABS recycled materials. DETAILED DESCRIPTION

[0025] The following embodiments of the present application will be described in detail with reference to the examples, but those skilled in the art will understand that the following examples are only used to illustrate the present application and should not be considered to limit the scope of the present application. If no specific conditions are specified in the examples, the conditions are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially. Organic antistatic agent: nylon 6 and ethylene oxide block copolymer is PEBAX MH2030 from Arkema.

[0026] Preparation Example 1 Preparation of ABS recycled material The ABS recycled material is recovered by a recycling method, comprising the following steps: S21, coarsely crushing the recovered ABS recycled material to obtain ABS recycled material fragments with a particle size of ≤30 mm; S22, performing preliminary cleaning on the ABS recycled material fragments, including pickling, rinsing and drying in sequence; S23, freezing the ABS recycled material after preliminary cleaning for 20 minutes, with the freezing temperature being -35°C; S24 finely grinds the frozen ABS recycled material to a particle size of 1-4 mm; washes the finely grinded ABS recycled material with a sodium chloride solution with a mass concentration of 6 g / L, rinses it after washing, and then dries it at 65° C. for 28 hours to obtain ABS recycled material.

[0027] Preparation Example 2 Preparation of polydopamine chemically grafted carbon nanotubes The preparation method of polydopamine chemically grafted carbon nanotubes comprises the following steps: S41, according to the mass fraction, placing 1 kg of carbon nanotubes in a mixed acid consisting of 7 kg of nitric acid with a mass concentration of 65% and 30 kg of sulfuric acid with a mass concentration of 98%, ultrasonically treating for 8 hours, cooling, diluting with deionized water, and filtering, washing the filter cake with distilled water to obtain hydroxylated carbon nanotubes; S42, according to the mass fractions, add 3 kg of γ-aminopropyltriethoxysilane and 0.25 kg of distilled water into a container and mix them evenly at room temperature, stir them thoroughly at room temperature, then slowly heat up to 50° C., react for 8 hours to obtain a colorless transparent liquid, and vacuum dry to obtain amino-terminated hyperbranched polysiloxane; S43. According to the mass fractions, 1.7 kg of polydopamine, 2.6 kg of amino-terminated hyperbranched polysiloxane and 0.8 kg of hydroxylated carbon nanotubes were added to 6 kg of isopropanol in a stirring state, and the mixture was stirred and mixed. Finally, ammonia water was added to adjust the pH value of the system to 7. The mixture was stirred for 3 hours, and then allowed to stand for 5 hours to obtain polydopamine chemically grafted carbon nanotubes.

[0028] Preparation Example 3 Preparation of polydopamine chemically grafted carbon nanotubes The preparation method of polydopamine chemically grafted carbon nanotubes comprises the following steps: S41, according to the mass fraction, placing 1 kg of carbon nanotubes in a mixed acid consisting of 7 kg of nitric acid with a mass concentration of 65% and 30 kg of sulfuric acid with a mass concentration of 98%, ultrasonically treating for 10 hours, cooling, diluting with deionized water, and filtering, washing the filter cake with distilled water to obtain hydroxylated carbon nanotubes; S42, according to the mass fractions, add 3 kg of γ-aminopropyltriethoxysilane and 0.3 kg of distilled water into a container and mix them evenly at room temperature, stir them thoroughly at room temperature, then slowly heat up to 55° C., react for 8 hours to obtain a colorless transparent liquid, and vacuum dry to obtain amino-terminated hyperbranched polysiloxane; S43. According to the mass fractions, 1.7 kg of polydopamine, 2.6 kg of amino-terminated hyperbranched polysiloxane and 1 kg of hydroxylated carbon nanotubes were added to 6 kg of isopropanol in a stirring state, and the mixture was stirred and mixed. Finally, ammonia water was added to adjust the pH value of the system to 8. The mixture was stirred for 2 h, and then allowed to stand for 4 h to obtain polydopamine chemically grafted carbon nanotubes.

[0029] Preparation Example 4 Preparation of polydopamine chemically grafted carbon nanotubes The preparation method of polydopamine chemically grafted carbon nanotubes comprises the following steps: S41, according to the mass fraction, placing 1 kg of carbon nanotubes in a mixed acid consisting of 7 kg of nitric acid with a mass concentration of 65% and 30 kg of sulfuric acid with a mass concentration of 98%, ultrasonically treating for 9 hours, cooling, diluting with deionized water, and filtering, washing the filter cake with distilled water to obtain hydroxylated carbon nanotubes; S42, according to the mass fractions, add 3 kg of γ-aminopropyltriethoxysilane and 0.28 kg of distilled water into a container and mix them evenly at room temperature, stir them thoroughly at room temperature, then slowly heat up to 53° C., react for 7 hours to obtain a colorless transparent liquid, and vacuum dry to obtain amino-terminated hyperbranched polysiloxane; S43. According to the mass fractions, 1.7 kg of polydopamine, 2.6 kg of amino-terminated hyperbranched polysiloxane and 0.9 kg of hydroxylated carbon nanotubes were added to 6 kg of isopropanol in a stirring state, and the mixture was stirred and mixed. Finally, ammonia water was added to adjust the pH value of the system to 7.5. The mixture was stirred for 2.5 h, and then allowed to stand for 4.5 h to obtain polydopamine chemically grafted carbon nanotubes.

[0030] Example 1 An antistatic ABS recycled material comprises the following raw materials, measured by weight: 90 kg of ABS recycled material, 5 kg of a composite antistatic agent, 4 kg of diphenylmethane diisocyanate, 2 kg of a coupling agent, and 0.3 kg of an antioxidant. The composite antistatic agent is prepared by mixing polydopamine chemically grafted carbon nanotubes and an organic antistatic agent in a weight ratio of 8:2, the coupling agent is composed of vinyltrichlorosilane, vinyltrimethoxysilane and γ-aminopropyltriethoxysilane in a weight ratio of 2:3:5, the antioxidant is composed of antioxidant 1010 and antioxidant 1076 in a weight ratio of 3:1, and the polydopamine chemically grafted carbon nanotubes are prepared according to Preparation Example 2.

[0031] The above-mentioned method for preparing an antistatic ABS recycled material comprises the following steps: S91. Evenly mix the ABS recycled material, the composite antistatic agent, the diphenylmethane diisocyanate, the coupling agent and the antioxidant in a high-speed mixer according to their weight fractions to obtain a mixture; S92. Feed the mixed material into a twin-screw extruder through an automatic feeding system for melt extrusion and granulation to obtain antistatic ABS recycled material. The twin-screw extruder comprises a first zone, a second zone, a third zone, a fourth zone, a fifth zone and a sixth zone connected in sequence, wherein the temperature of the first zone is 170°C, the temperature of the second zone is 170°C, the temperature of the third zone is 180°C, the temperature of the fourth zone is 180°C, the temperature of the fifth zone is 180°C, and the temperature of the sixth zone is 180°C.

[0032] Example 2 An antistatic ABS recycled material comprises the following raw materials, measured by weight: 95 kg of ABS recycled material, 7 kg of a composite antistatic agent, 5 kg of diphenylmethane diisocyanate, 3 kg of a coupling agent, and 0.4 kg of an antioxidant. The composite antistatic agent is prepared by mixing polydopamine chemically grafted carbon nanotubes and an organic antistatic agent in a weight ratio of 8:3, the coupling agent is composed of vinyltrichlorosilane, vinyltrimethoxysilane and γ-aminopropyltriethoxysilane in a weight ratio of 2:3:5, the antioxidant is composed of antioxidant 1010 and antioxidant 1076 in a weight ratio of 3:1, and the polydopamine chemically grafted carbon nanotubes are prepared in Preparation Example 3.

[0033] The above-mentioned method for preparing an antistatic ABS recycled material comprises the following steps: S91. Evenly mix the ABS recycled material, the composite antistatic agent, the diphenylmethane diisocyanate, the coupling agent and the antioxidant in a high-speed mixer according to their weight fractions to obtain a mixture; S92. Feed the mixed material into a twin-screw extruder through an automatic feeding system for melt extrusion and granulation to obtain antistatic ABS recycled material. The twin-screw extruder comprises a first zone, a second zone, a third zone, a fourth zone, a fifth zone and a sixth zone which are connected in sequence, wherein the temperature of the first zone is 180°C, the temperature of the second zone is 180°C, the temperature of the third zone is 190°C, the temperature of the fourth zone is 190°C, the temperature of the fifth zone is 190°C, and the temperature of the sixth zone is 190°C.

[0034] Example 3 An antistatic ABS recycled material comprises the following raw materials, measured by weight: 93 kg of ABS recycled material, 6 kg of a composite antistatic agent, 4.5 kg of diphenylmethane diisocyanate, 2.5 kg of a coupling agent, and 0.35 kg of an antioxidant. The composite antistatic agent is prepared by mixing polydopamine chemically grafted carbon nanotubes and an organic antistatic agent in a weight ratio of 8:2.5. The coupling agent is composed of vinyltrichlorosilane, vinyltrimethoxysilane and γ-aminopropyltriethoxysilane in a weight ratio of 2:3:5. The antioxidant is composed of antioxidant 1010 and antioxidant 1076 in a weight ratio of 3:1. The polydopamine chemically grafted carbon nanotubes are prepared according to Preparation Example 4.

[0035] The above-mentioned method for preparing an antistatic ABS recycled material comprises the following steps: S91. Evenly mix the ABS recycled material, the composite antistatic agent, the diphenylmethane diisocyanate, the coupling agent and the antioxidant in a high-speed mixer according to their weight fractions to obtain a mixture; S92. Feed the mixed material into a twin-screw extruder through an automatic feeding system for melt extrusion and granulation to obtain antistatic ABS recycled material. The twin-screw extruder comprises a first zone, a second zone, a third zone, a fourth zone, a fifth zone and a sixth zone which are connected in sequence, wherein the temperature of the first zone is 175°C, the temperature of the second zone is 175°C, the temperature of the third zone is 185°C, the temperature of the fourth zone is 185°C, the temperature of the fifth zone is 185°C, and the temperature of the sixth zone is 185°C.

[0036] Comparative Example 1 The same as Example 3, except that an equal amount of carbon nanotubes is used to replace the polydopamine chemically grafted carbon nanotubes.

[0037] Comparative Example 2 The same as Example 3, except that an equal amount of polydopamine chemically grafted carbon nanotubes is used instead of the composite antistatic agent.

[0038] Comparative Example 3 The same as Example 3, except that an equal amount of organic antistatic agent is used instead of the composite antistatic agent.

[0039] Comparative Example 4 The same as Example 3, except that the coupling agent is vinyltrichlorosilane.

[0040] Comparative Example 5 The same as Example 3, except that the coupling agent is vinyltrimethoxysilane.

[0041] Comparative Example 6 The same as Example 3, except that the coupling agent is γ-aminopropyltriethoxysilane.

[0042] Comparative Example 7 The same as Example 3, except that the amount of diphenylmethane diisocyanate added was 0 kg.

[0043] Performance Testing The antistatic ABS recycled materials prepared in Examples 1 to 3 and Comparative Examples 1 to 7 were sampled and injection molded into test bars, and the following performance tests were performed. The test results are shown in Table 1; Surface resistance: refer to GB / T1410-2006, test 3mm thick square plate; Notched impact strength: tested in accordance with GB / T1843-1996; sample size is 80×10×4mm, notch depth is 2mm; Tensile strength and elongation at break: tested in accordance with GB / T10470-1992 standard, sample size is 150×10×4mm, tensile rate is 50mm / min.

[0044] Table 1 Performance test Analyzing the data in Table 1, we can see that: 1) The antistatic ABS recycled materials obtained in Examples 1 to 3 have excellent antistatic properties and mechanical properties, and can meet application scenarios with high standards and long-term antistatic requirements.

[0045] 2) The performance comparison analysis of the antistatic ABS recycled materials prepared in combination with Example 3 and Comparative Example 1 shows that after polydopamine is chemically grafted onto carbon nanotubes, the high conductivity of carbon nanotubes and the charge transfer characteristics of polydopamine can be used to effectively improve the antistatic properties of ABS recycled materials. Carbon nanotubes themselves have extremely high strength and modulus. After being grafted into ABS recycled materials, the mechanical properties of the material, especially tensile properties and impact strength, can be significantly improved. Improve compatibility and dispersibility: amino-terminated hyperbranched polysiloxane is used as a coupling agent to help improve the dispersibility of carbon nanotubes in the ABS matrix, reduce agglomeration, and increase the interfacial interaction between carbon nanotubes and ABS, thereby improving the overall performance of the material.

[0046] 3) The performance comparison analysis of the antistatic ABS recycled materials prepared in combination with Example 3 and Comparative Examples 2-3 shows that the composite antistatic agent is prepared by mixing polydopamine chemically grafted carbon nanotubes and organic antistatic agents in a mass ratio of 8:2-3. By compounding polydopamine chemically grafted carbon nanotubes and organic antistatic agents, excellent antistatic performance can be achieved at a lower addition amount, thereby reducing the amount of antistatic agent. The synergistic effect between polydopamine chemically grafted carbon nanotubes and organic antistatic agents improves the compatibility between the composite antistatic agent and ABS recycled materials, and at the same time improves the dispersibility of the antistatic agent in ABS recycled materials. The synergistic effect of the composite antistatic agent improves the antistatic efficiency of the antistatic ABS recycled materials, thereby meeting the application scenarios with high standards and long-term antistatic requirements. The synergistic effect between polydopamine chemically grafted carbon nanotubes and organic antistatic agents can enable the composite antistatic agent to achieve excellent antistatic properties at a lower addition amount, reduce production costs, and improve the mechanical properties of antistatic ABS recycled materials, thereby meeting a wider range of application needs.

[0047] 4) The performance comparison analysis of the antistatic ABS recycled materials prepared in combination with Example 3 and Comparative Examples 4-6 shows that the coupling agent is composed of vinyl trichlorosilane, vinyl trimethoxysilane and γ-aminopropyl triethoxysilane in a mass ratio of 2:3:5. By utilizing the synergistic effect between them, the compatibility and dispersibility between the antistatic agent and the ABS recycled materials can be improved, thereby improving the mechanical properties (such as impact strength) and antistatic efficiency of the antistatic ABS recycled materials. Vinyl trichlorosilane, vinyl trimethoxysilane and γ-aminopropyl triethoxysilane work synergistically to tightly combine the antistatic agent with the ABS recycled materials through chemical bonding to form a stable composite material. This structure not only improves the dispersibility of the antistatic agent in the ABS recycled materials, but also enhances the interaction between the antistatic agent and the ABS recycled materials, thereby improving the overall performance of the antistatic ABS recycled materials. In addition, these coupling agents can also repair the broken chains in the ABS recycled materials, further improving their mechanical properties.

[0048] 5) The comparative analysis of the performance of the antistatic ABS recycled materials obtained in Example 3 and Comparative Example 7 shows that the introduction of diphenylmethane diisocyanate improves the viscosity and molecular weight of the antistatic ABS recycled material, repairs the broken chains in the ABS recycled material, improves the mechanical properties, and especially significantly improves the tensile properties.

[0049] The above embodiments are only used to explain the technical solutions of the present application rather than to limit them. Although the above embodiments provide a specific description of the present application, relevant technical personnel should understand that the specific implementation modes of the present invention can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present application should be included in the scope of protection of the present application.

Claims

1. An antistatic ABS recycled material, characterized in that: The preparation raw materials include the following by weight: 90-95 parts of ABS recycled materials, 5-7 parts of composite antistatic agent, 4-5 parts of diphenylmethane diisocyanate, 2-3 parts of coupling agent and 0.3-0.4 parts of antioxidant.

2. The antistatic ABS recycled material according to claim 1, characterized in that: The ABS recycled material is recovered by a recycling method, and the recycling method comprises the following steps: S21, coarsely crushing the recovered ABS recycled material to obtain ABS recycled material fragments with a particle size of ≤30 mm; S22, performing preliminary cleaning on the ABS recycled material fragments, including pickling, rinsing and drying in sequence; S23, freezing the ABS recycled material after preliminary cleaning for 10-30 minutes, with the freezing temperature being -40°C to -20°C; S24 finely grinds the frozen ABS recycled material to a particle size of 1-4 mm; washes the finely grinded ABS recycled material with a sodium chloride solution with a mass concentration of 5.5-6.5 g / L, rinses it after washing, and then dries it at 60-70° C. for 20-36 hours to obtain ABS recycled material.

3. The antistatic ABS recycled material according to claim 1, characterized in that: The composite antistatic agent is prepared by mixing polydopamine chemically grafted carbon nanotubes and an organic antistatic agent in a mass ratio of 8:2-3.

4. The antistatic ABS recycled material according to claim 3, characterized in that: The method for preparing polydopamine chemically grafted carbon nanotubes comprises the following steps: S41, placing 10 parts of carbon nanotubes in a mixed acid consisting of 70 parts of nitric acid with a mass concentration of 65% and 30 parts of sulfuric acid with a mass concentration of 98%, ultrasonically treating for 8-10 hours, cooling, diluting with deionized water, and filtering, washing the filter cake with distilled water to obtain hydroxylated carbon nanotubes; S42, according to the mass fractions, add 30 parts of γ-aminopropyltriethoxysilane and 2.5-3 parts of distilled water into a container and mix them evenly at room temperature, stir them thoroughly at room temperature, then slowly heat up to 50-55° C., react for 5-8 hours to obtain a colorless transparent liquid, and vacuum dry to obtain amino-terminated hyperbranched polysiloxane; S43. According to the mass fractions, add polydopamine, amino-terminated hyperbranched polysiloxane and hydroxylated carbon nanotubes to isopropanol in sequence under stirring, stir and mix, and finally add ammonia water to adjust the pH of the system to 7-8, continue stirring for 2-3 hours, and then let it stand for 4-5 hours to obtain polydopamine chemically grafted carbon nanotubes.

5. The antistatic ABS recycled material according to claim 4, characterized in that: In step S43, the mass ratio of the isopropanol, polydopamine, amino-terminated hyperbranched polysiloxane and hydroxylated carbon nanotubes is 60:17:26:(8-10).

6. The antistatic ABS recycled material according to claim 3, characterized in that: The organic antistatic agent is a block copolymer of nylon 6 and ethylene oxide.

7. The antistatic ABS recycled material according to claim 1, characterized in that: The coupling agent is composed of vinyl trichlorosilane, vinyl trimethoxysilane and gamma-aminopropyl triethoxysilane in a mass ratio of 2:3:

5.

8. The antistatic ABS recycled material according to claim 1, characterized in that: The antioxidant is composed of antioxidant 1010 and antioxidant 1076 in a mass ratio of 3:

1.

9. A method for preparing an antistatic ABS recycled material according to any one of claims 1 to 8, characterized in that: The following steps are involved: S91. Evenly mix the ABS recycled material, the composite antistatic agent, the diphenylmethane diisocyanate, the coupling agent and the antioxidant in a high-speed mixer according to their weight fractions to obtain a mixture; S92, feeding the mixed material into a twin-screw extruder through an automatic feeding system for melt extrusion and granulation to obtain antistatic ABS recycled material.

10. The method for preparing antistatic ABS recycled material according to claim 9, characterized in that: The twin-screw extruder comprises a first zone, a second zone, a third zone, a fourth zone, a fifth zone and a sixth zone which are connected in sequence, wherein the temperature of the first zone is 170-180°C, the temperature of the second zone is 170-180°C, the temperature of the third zone is 180-190°C, the temperature of the fourth zone is 180-190°C, the temperature of the fifth zone is 180-190°C, and the temperature of the sixth zone is 180-190°C.

Citation Information

Patent Citations

  • A novel antistatic ABS resin material and its preparation method

    CN102268171A

  • Novel antistatic ABS composite material and preparation method thereof

    CN110615953A

Cited By

  • Antistatic flame-retardant material as well as preparation method and application thereof

    CN120209391A