ABS composite material, preparation method thereof and appearance ornament
By combining ABS resin, MS-NB, MBS, titanium dioxide and PA66, PA6 and other materials in ABS composite materials, the ink flow pattern appearance effect and good mechanical properties are achieved, and the spraying and transfer processes in the prior art are solved. Environmental and cost issues, suitable for the production of high-quality decorative parts for automotive interiors.
Patent Information
- Application Number
- CN202411389273.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-12-06
AI Technical Summary
The spraying and transfer printing process of existing automotive interior decorative parts has poor environmental friendliness, many production links, low efficiency, high cost, and poor recycling, which affects reuse.
Using ABS composite material, the particles of ABS resin, MS-NB, MBS, titanium dioxide and PA66, PA6, inorganic filler, solvent blue, solvent red and other compositions are mixed in a specific proportion, and the ink flow pattern is achieved by injection molding. Effects, while ensuring mechanical properties.
It realizes the appearance effect of ink and wash, improves the experience of the car interior, and has good comprehensive performance such as impact resistance, heat resistance, high toughness, etc., reduces production costs, simplifies the process flow, and reduces the emission of volatile substances. .
Smart Images

Figure BDA0005073352510000091 
Figure HDA0005073352620000011 
Figure HDA0005073352620000012
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of materials, and in particular to an ABS composite material and a preparation method and appearance decoration thereof. Background Art
[0002] As people's living standards improve, their consumption levels also upgrade. Consumers define automobiles as mobile private spaces to a large extent, which leads to consumers paying more attention to the quality of interior decoration. And as the consumer market loves simple and textured car cabins, car interiors tend to be designed with some special high-quality textures.
[0003] Car interior decoration is one of the important means to improve the visual effect of the car interior and enhance the quality of the whole car. In order to achieve the special texture effect of the car interior decoration, it is usually necessary to process the plastic parts through secondary processing such as painting and transfer. However, the spraying and transfer processes are not environmentally friendly, have many production links, low efficiency, and high overall costs. In addition, the plastic products after spraying and transfer have poor recyclability, which affects their reuse. Summary of the invention
[0004] The present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, one object of the present invention is to provide an ABS composite material, which can have the appearance effect of ink flow lines.
[0005] In one aspect of the present invention, the present invention provides an ABS composite material. According to an embodiment of the present invention, the ABS composite material comprises first composition particles and second composition particles, wherein the first composition particles comprise ABS resin, MS-NB, MBS, titanium dioxide and lubricant, and the second composition particles comprise PA66, PA6, inorganic filler, solvent blue and solvent red. Therefore, the ABS composite material of the above composition can effectively achieve the appearance effect of ink-water rippling, improve the experience of automobile interior decoration, and ensure its good mechanical properties, that is, it has balanced physical and mechanical properties and a wide processing window. Specifically: in the ABS composite material, ABS resin can provide excellent heat resistance and high elastic toughness for the composite material, MS-NB can further provide good heat resistance for the composite material, improve its overall heat deformation temperature, and MBS can provide good impact resistance for the composite material. Therefore, the ABS composite material of the present invention has good comprehensive properties such as impact resistance, heat resistance, and high toughness; with the help of titanium dioxide to ensure the base color of the composite material, PA66 and PA6 combined resins are used as the carrier resin of the masterbatch, and the solvent red and solvent blue are compounded to achieve a three-dimensional ink-water rippling effect on the product surface; the melting point difference between the carrier resin (PA66 and PA6) of the masterbatch and the ABS resin substrate makes it have different melting states during the injection molding process, thereby reflecting the ink texture effect in the ABS resin substrate with a white base; further, the ABS composite material of the present invention has a lower glossiness and is more suitable for manufacturing automobile interior decoration products.
[0006] According to an embodiment of the present invention, based on the total weight of the first composition particles, the first composition particles include, by mass percentage: 69 to 83.8 wt% of the ABS resin; 8 to 12 wt% of the MS-NB; 3 to 8 wt% of the MBS; 5 to 10 wt% of the titanium dioxide; and 0.2 to 1 wt% of the lubricant; based on the total weight of the second composition particles, by mass percentage, the second composition particles include: 52 to 76 wt% of the PA66 resin; 20 to 30 wt% of the PA6 resin; 3 to 15 wt% of the inorganic filler; 0.5 to 1.5 wt% of the solvent blue; and 0.5 to 1.5 wt% of the solvent red.
[0007] According to an embodiment of the present invention, the mass mixing ratio of the first composition particles to the second composition particles is 95:5 to 70:30.
[0008] According to an embodiment of the present invention, the melt mass flow rate of the ABS resin is 5 to 10 g / 10 min.
[0009] According to an embodiment of the present invention, the ABS composite material further satisfies at least one of the following conditions: the lubricant includes at least one of PETS, EBS, zinc stearate and montan acid wax; the inorganic filler includes wollastonite; the aspect ratio of the inorganic filler is 1 to 3; the solvent blue is solvent blue 104, and the solvent red is solvent red 207.
[0010] The glossiness of the ABS composite material according to the embodiment of the present invention is 35-50GU; the heat deformation temperature is 80-90°C; and the notched impact is 9-15KJ / m 2 ; The tensile strength is 46~65MPa.
[0011] In another aspect of the present invention, the present invention provides a method for preparing the aforementioned ABS composite material. According to an embodiment of the present invention, the method for preparing the ABS composite material comprises: mixing the first composition particles and the second composition particles according to a predetermined ratio to obtain mixed particles; and injection molding the mixed particles to obtain the ABS composite material. Thus, directly preparing the ABS composite material by injection molding can achieve an appearance effect similar to transfer printing and spraying, but compared with transfer printing and spraying technology, the preparation method of the present invention is simpler and has lower cost, which is conducive to reducing the emission of volatile substances, and at the same time can meet the use requirements of automotive interiors.
[0012] According to an embodiment of the present invention, the preparation method of the first composition particles includes: stirring the raw materials of the first composition particles at high speed for a first premixing to obtain a first mixture; adding the first mixture through the main feeding port of the twin-screw extruder, and undergoing a first melt blending, cooling and granulation to obtain the first composition particles. The preparation method of the second composition particles includes: stirring the raw materials of the second composition particles at high speed for a second premixing to obtain a second mixture; adding the second mixture through the main feeding port of the twin-screw extruder, and undergoing a second melt blending, cooling and granulation to obtain the second composition particles.
[0013] According to an embodiment of the present invention, the mixing temperature of the first premixing and the second premixing is not higher than 60°C, the stirring speed is 800-1200r / min, and the mixing time is 1-2min; during the first melt blending process, the temperature is 190-230°C, and the screw speed of the twin-screw extruder main machine is 500-600r / min; during the second melt blending process, the temperature is 200-250°C, and the screw speed of the twin-screw extruder main machine is 500-600r / min.
[0014] In another aspect of the present invention, an exterior decoration is provided. According to an embodiment of the present invention, the exterior decoration comprises the ABS composite material described above. Thus, the exterior decoration has the appearance effect of ink-and-wash rhymes, which can improve the experience of the car interior, and at the same time has good mechanical properties such as heat resistance, strong impact resistance, and high elastic toughness. It can be understood by those skilled in the art that the exterior decoration has all the characteristics and advantages of the ABS composite material described above, and no further elaboration is given here. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0016] Figure 1 This is a photo of the ABS composite material prepared in Example 1 of the present invention;
[0017] Figure 2 This is a photo of the ABS composite material prepared in Example 2 of the present invention;
[0018] Figure 3 This is a photo of the ABS composite material prepared in Example 3 of the present invention;
[0019] Figure 4 This is a photo of the ABS composite material prepared in Example 4 of the present invention;
[0020] Figure 5 This is a photo of the ABS composite material prepared in Example 5 of the present invention;
[0021] Figure 6 This is a photo of the ABS composite material prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0022] The scheme of the present invention will be explained below in conjunction with the embodiments. It will be appreciated by those skilled in the art that the following embodiments are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. Where specific techniques or conditions are not indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used are not indicated by the manufacturer and are all conventional products that can be obtained commercially.
[0023] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.
[0024] In one aspect of the present invention, the present invention provides an ABS composite material. According to an embodiment of the present invention, the ABS composite material includes a first composition particle and a second composition particle, wherein the first composition particle includes ABS resin (acrylonitrile-styrene-butadiene copolymer), MS-NB (styrene-N-phenylmaleimide-anhydrous maleic acid copolymer), MBS (terpolymer of methyl methacrylate-butadiene-styrene), titanium dioxide and lubricant, and the second composition particle includes PA66 (polyhexamethylene adipamide, commonly known as nylon-66), PA6 (nylon 6, also known as polyamide 6), inorganic filler, solvent blue and solvent red. Therefore, the ABS composite material of the above composition can effectively achieve the appearance effect of ink-water rippling, improve the experience of automobile interior decoration, and ensure its good mechanical properties, that is, it has balanced physical and mechanical properties and a wide processing window. Specifically: in the ABS composite material, ABS resin can provide excellent heat resistance and high elastic toughness for the composite material, MS-NB can further provide good heat resistance for the composite material, improve its overall heat deformation temperature, and MBS can provide good impact resistance for the composite material. Therefore, the ABS composite material of the present invention has good comprehensive properties such as impact resistance, heat resistance, and high toughness; with the help of titanium dioxide to ensure the base color of the composite material, PA66 and PA6 combined resins are used as the carrier resin of the masterbatch, and the solvent red and solvent blue are compounded to achieve a three-dimensional ink-water rippling effect on the product surface; the melting point difference between the carrier resin (PA66 and PA6) of the masterbatch and the ABS resin substrate makes it have different melting states during the injection molding process, thereby reflecting the ink texture effect in the ABS resin substrate with a white base; further, the ABS composite material of the present invention has a lower glossiness and is more suitable for manufacturing automobile interior decoration products.
[0025] According to an embodiment of the present invention, based on the total weight of the first composition particles, the first composition particles include, by mass percentage: 69-83.8wt% of ABS resin (for example, 69wt%, 70wt%, 73wt%, 76.5wt%, 78wt%, 80wt%, 83.5wt%, 83.8wt%, etc.); 8-12wt% of MS-NB (for example, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, etc.); 3-8wt% of MBS (for example, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, etc.); 5-10wt% of titanium dioxide (for example, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, etc.); and 0.2-1wt% of lubricant (for example, 0.2wt%, 0.5wt%, 0.8wt%, 1.0wt%, etc.).
[0026] According to an embodiment of the present invention, based on the total weight of the second composition particles, the second composition particles include, by mass percentage: 52-76wt% of PA66 resin (for example, 52wt%, 55wt%, 60wt%, 63wt%, 65wt%, 70wt%, 76wt%, etc.); 20-30wt% of PA6 resin (for example, 20wt%, 22wt%, 25wt%, 28wt%, 30wt%, etc.); 3-15wt% of inorganic filler (for example, 3wt%, 5wt%, 7wt%, 8wt%, 10wt%, 13wt%, 15wt%, etc.); 0.5-1.5wt% of solvent blue (for example, 0.5wt%, 0.8wt%, 1.0wt%, 1.2wt%, 1.5wt%, etc.); and 0.5-1.5wt% of solvent red (for example, 0.5wt%, 0.8wt%, 1.0wt%, 1.2wt%, 1.5wt%, etc.). Therefore, the ABS composition obtained by the above ratio can ensure its good ink-and-water appearance effect while ensuring its good comprehensive properties such as impact resistance, heat resistance, and high toughness.
[0027] According to an embodiment of the present invention, the mass mixing ratio of the first composition particles and the second composition particles is 95:5 to 70:30. For example, the mass mixing ratio of the first composition particles and the second composition particles is 95:5, 90:10, 85:15, 80:20, 75:25, 70:30, etc. The above ratios can ensure that an ABS composite material with excellent appearance and performance is obtained.
[0028] In some embodiments of the present invention, the melt mass flow rate (melt index) of the ABS resin is 5 to 10 g / 10 min, such as 5 g / 10 min, 6 g / 10 min, 7 g / 10 min, 8 g / 10 min, 9 g / 10 min, 10 g / 10 min, etc. The suitable melt mass flow rate of the ABS resin of the present invention can well balance the mechanical properties of the ABS composite material and the smooth implementation of injection molding (ensuring that the melt filling mold process can be achieved slowly and stably). If the melt mass flow rate of the ABS resin is low, the mechanical properties of the composite material are affected; if the melt mass flow rate of the ABS resin is too high, the flow stability of the material during the injection molding process will be worse, which is not conducive to achieving the flow pattern effect of the final product.
[0029] In some embodiments of the present invention, the crystal form of titanium dioxide includes rutile. Therefore, titanium dioxide is used to ensure the base color of the composite material, and the covering power of rutile titanium dioxide will be higher. Adding it to the material system can make the ABS composite material have a better visual effect. Moreover, the influence of rutile titanium dioxide on the physical and mechanical properties of the composite material will be smaller, which will help to further ensure the good physical and mechanical properties of the composite material such as heat resistance, impact resistance, and high toughness. Among them, the titanium dioxide in the composite material of the present invention can be all rutile titanium dioxide, or most of the titanium dioxide (such as 60%, 70% or even more than 80% of the titanium dioxide) is rutile titanium dioxide, and a small amount is titanium dioxide of other crystal forms.
[0030] In some embodiments of the present invention, the lubricant includes at least one of PETS, EBS, zinc stearate and montan acid wax. The above lubricants can well ensure good processability of the first composition particles and dispersibility of titanium dioxide.
[0031] In some embodiments of the present invention, PA66 and PA6 can be used as good masterbatch carriers for solvent blue and solvent red for the following reasons: first, the melting point of PA6 is about 230°C, the melting point of PA66 is about 260°C, and the processing temperature of a common ABS resin is about 220°C, that is, the melting points of PA66 and PA6 are higher than the processing temperature of ABS resin, so the PA66 and PA6 masterbatch carriers are in a semi-molten state during processing, ensuring that the flow effect in the masterbatch carriers PA66 and PA6 will not be fully dispersed in the matrix, thereby showing a faint flow effect on the composite material; second, selecting two nylon resins, PA66 and PA6, as masterbatch carriers ensures the dissolution gradient of the toner, and the appearance effect can be adjusted by adjusting the ratio of PA6 to PA66. If PA6 or PA66 is selected as the masterbatch carrier substrate alone, the processing window of the composite material will be narrower, and it will be difficult to stably achieve the target ink flow effect in actual production; thirdly, the solubility parameters between A6 and PA66 and the ABS substrate are quite different, and they are not a good compatible system. Therefore, it will bring a natural matte effect to the product composite material, which will make the final product more visually textured.
[0032] In some embodiments of the present invention, the inorganic filler includes wollastonite, and the aspect ratio of the inorganic filler is 1 to 3, such as 1, 1.5, 2, 2.5, and 3. Therefore, the wollastonite with the above aspect ratio can better play a disturbing role on the color powders such as solvent blue and solvent red during the injection molding process of the composite material, ensuring that the flow direction of the dye in the second composite material particles has no clear regularity, thereby forming a good rhytidal ink effect; moreover, the wollastonite with the above aspect ratio has a relatively small effect on the mechanical properties of the ABS resin substrate. If the aspect ratio is too long, it will affect the toughness of the material. If the aspect ratio of the inorganic filler is too short, the disturbing effect on the color powder is weak, and even the disturbing effect cannot be achieved.
[0033] In some embodiments of the present invention, the solvent blue is solvent blue 104, and the solvent red is solvent red 207. The above two dyes are compounded and colored on PA66 and PA6 resins, and under the comprehensive effect of other components, a three-dimensional ink flow pattern effect is formed on the surface of the composite material.
[0034] According to an embodiment of the present invention, the glossiness of the ABS composite material of the present invention is 35 to 50GU, such as 35GU, 37GU, 40GU, 42GU, 45GU, 47GU, 50GU, etc.; the heat deformation temperature is 80 to 90°C, such as 80°C, 82°C, 84°C, 85°C, 88°C, 90°C, etc.; the notched impact is 9 to 15KJ / m 2 , for example 9KJ / m 2 、10KJ / m 2 、11KJ / m 2 、12KJ / m 2 、13KJ / m 2 、14KJ / m 2 、15KJ / m 2 The tensile strength is 46-65MPa, such as 46MPa, 47MPa, 48MPa, 49MPa, 50MPa, 52MPa, 55MPa, 57MPa, 60MPa, etc. It can be seen that the ABS composite material of the present invention has relatively excellent heat resistance and impact resistance, has lower glossiness, can better meet the requirements of automotive accessories, and improve its experience and visual effects.
[0035] In another aspect of the present invention, the present invention provides a method for preparing the above-mentioned ABS composite material. According to an embodiment of the present invention, the method for preparing the ABS composite material comprises:
[0036] S100: mixing the first composition particles and the second composition particles according to a predetermined ratio to obtain mixed particles;
[0037] In some embodiments, the mass mixing ratio of the first composition particles and the second composition particles is 95:5 to 70:30. For example, the mass mixing ratio of the first composition particles and the second composition particles is 95:5, 90:10, 85:15, 80:20, 75:25, 70:30, etc. The above ratios can ensure that an ABS composite material with better appearance and performance is obtained.
[0038] According to some embodiments of the present invention, the preparation method of the first composite particle comprises: stirring the raw materials of the first composite particle, such as ABS resin, MS-NB, MBS, titanium dioxide and lubricant, at high speed for first premixing to obtain a first mixture; adding the first mixture through the main feed port of a twin-screw extruder, and undergoing first melt blending, cooling and granulation to obtain the first composite particle. Further, in some embodiments, the mixing temperature of the first premix is not higher than 60°C, the stirring speed is 800-1200r / min, and the mixing time is 1-2min; during the first melt blending process, the temperature is 190-230°C, and the screw speed of the twin-screw extruder main engine is 500-600r / min.
[0039] According to some embodiments of the present invention, the preparation method of the second composite particle comprises: stirring the raw materials of the second composite particle such as PA66, PA6, inorganic filler, solvent blue and solvent red at high speed for second premixing to obtain a second mixture; adding the second mixture through the main feeding port of the twin-screw extruder, and undergoing second melt blending, cooling and granulation to obtain the second composite particle. Further, in some embodiments, according to the embodiments of the present invention, the mixing temperature of the first premixing and the second premixing is not higher than 60°C (effectively ensuring that the dye toner selected in the second premixing stage does not melt, so as not to reduce its dispersion effect), the stirring speed is 800-1200r / min, and the mixing time is 1-2min; during the first melt blending process, the temperature is 190-230°C, and the screw speed of the twin-screw extruder main engine is 500-600r / min; during the second melt blending process, the temperature is 200-250°C, and the screw speed of the twin-screw extruder main engine is 500-600r / min.
[0040] S200: The mixed particles are injection molded to obtain an ABS composite material.
[0041] According to some embodiments of the present invention, during the injection molding process, the heating temperature of the heating section (including the front section, the middle section and the rear section) is 200° C. to 230° C. Thus, a composite material with excellent appearance and mechanical properties can be obtained by injection molding.
[0042] In some embodiments, before injection molding, the mixed particles may be dried in advance, for example, by using a non-blast oven to fully dry the mixed particles to remove moisture from the mixed particles.
[0043] According to the embodiments of the present invention, the ABS composite material is directly prepared by injection molding, that is, the appearance effect of ink-water rippling similar to transfer printing and spraying can be achieved, but relative to the transfer printing and spray printing technology, the preparation method of the present invention is simpler, has lower cost, and is conducive to reducing the emission of volatile substances, while meeting the use requirements of automobile interiors. At the same time, the ABS composite material of the present invention can effectively achieve the appearance effect of ink-water rippling, can improve the experience of automobile interiors, and at the same time ensure its good mechanical properties, that is, it has balanced physical and mechanical properties and a wide processing window. At the same time, the prepared ABS composite material has a lower glossiness and is more suitable for manufacturing automobile interior products.
[0044] In another aspect of the present invention, an exterior decoration is provided. According to an embodiment of the present invention, the exterior decoration comprises the ABS composite material described above. Thus, the exterior decoration has the appearance effect of ink-and-wash rhyme, has a lower glossiness, can improve the experience of the car interior, and at the same time has good mechanical properties such as heat resistance, strong impact resistance, and high elastic toughness. It can be understood by those skilled in the art that the exterior decoration has all the characteristics and advantages of the ABS composite material described above, and no further elaboration is given here.
[0045] According to some embodiments of the present invention, the exterior decoration may be a product for automobile interior decoration, having a three-dimensional ink-and-wash flow pattern appearance effect and a lower glossiness, which can greatly improve the automobile experience.
[0046] Example
[0047] Example 1
[0048] 1) Preparation method of the first composite particle:
[0049] Raw materials provided: ABS resin (ABS8391, Gaoqiao Petrochemical) 76.5wt%, MS-NB (IP30009, Electrochemical) 10wt%, MBS (EM500, LG Chemical) 5wt%, titanium dioxide (R108, DuPont) 8%, lubricant (PETS, Lonza) 0.5wt%.
[0050] After the above components are premixed in a high-speed mixer, they are added from the main feeding port of a twin-screw extruder to obtain first composite particles through melt blending, stranding, water cooling, pelletizing and drying.
[0051] 2) Preparation method of the second composition particles:
[0052] Raw materials provided: PA66 resin (EPR27, Shenma) 63wt%, PA6 resin (M2400, Xinhui Mei Da) 25%, wollastonite (SW-18, wollastonite) 10wt%, solvent blue 104 (McLean) 1wt%, solvent red 207 (McLean) 1wt%.
[0053] After the above components are premixed in a high-speed mixer, they are added from the main feeding port of a twin-screw extruder to obtain the second composition particles through melt blending, stranding, water cooling, pelletizing and drying.
[0054] 3) The first composite particles and the second composite particles prepared according to the above formula are mixed in a mass ratio of 95:5, dried, and injection molded to obtain an ABS composite material. The actual photo can be referred to Figure 1 .
[0055] Example 2
[0056] The difference from Example 1 is that the mass ratio of the first composite particle to the second composite particle is 70:30. The actual photo of the obtained ABS composite material can be referred to Figure 2 .
[0057] Example 3
[0058] The difference from Example 1 is that the mass ratio of the first composite particle to the second composite particle is 80:20. The actual photo of the obtained ABS composite material can be referred to Figure 3 .
[0059] Example 4
[0060] The difference from Example 1 is that the mass ratio of the first composite particle to the second composite particle is 97:3. The actual photo of the obtained ABS composite material can be referred to Figure 4 .
[0061] Example 5
[0062] The difference from Example 1 is that the mass ratio of the first composite particle to the second composite particle is 65:35. The actual photo of the obtained ABS composite material can be referred to Figure 5 .
[0063] Comparative Example 1
[0064] The raw materials include ABS resin (ABS3504, Gaoqiao Petrochemical) 92wt%, titanium dioxide (R108, DuPont) 8%. After the above components are pre-mixed in a high-speed mixer, they are added from the main feed port of a twin-screw extruder, and ABS material is obtained through melt blending, stranding, water cooling, pelletizing, and drying. The ABS material is fully dried and injection molded to obtain a comparative composite material. The actual photo can be referred to Figure 6 .
[0065] The performance tests were performed on the composite materials obtained in Examples 1 to 5 and Comparative Example 1, as shown in Table 1.
[0066] Table 1
[0067]
[0068] It can be seen from the test results in Table 1 that the ABS composite material of the present invention not only has an appearance effect of showing three-dimensional ink-water flow patterns, but also has better heat resistance, impact resistance and tensile strength in terms of physical and mechanical properties, and has lower glossiness, and can be suitable for automotive interior decoration.
[0069] According to the actual photos of the composite materials of Examples 1 to 5, it can be seen that the composite materials of Examples 1 to 3 have a smoother and three-dimensional appearance of ink flow patterns. Combined with the performance test in Table 1, it is shown that when the mixing ratio of the first composition particles to the second composition particles is 95:5 to 70:30, the appearance effect and mechanical properties of the obtained composite materials are better.
[0070] The terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0071] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, unless they are contradictory.
[0072] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. An ABS composite material, characterized in that: The invention comprises particles of a first composition and particles of a second composition, wherein the particles of the first composition comprise ABS resin, MS-NB, MBS, titanium dioxide and lubricant, and the particles of the second composition comprise PA66, PA6, inorganic filler, solvent blue and solvent red.
2. The ABS composite material according to claim 1, characterized in that: Based on the total weight of the first composition particles, the first composition particles include, by mass percentage: The ABS resin is 69-83.8wt%; The MS-NB 8 to 12 wt%; The MBS 3-8wt%; 5 to 10 wt% of the titanium dioxide; and The lubricant is 0.2-1 wt%, Based on the total weight of the second composition particles, the second composition particles include, by mass percentage: The PA66 resin 52-76wt%; 20-30wt% of PA6 resin; The inorganic filler is 3 to 15 wt%; 0.5-1.5 wt% of the solvent blue; and The solvent red is 0.5-1.5 wt%.
3. The ABS composite material according to claim 1, characterized in that: The mass mixing ratio of the first composition particles to the second composition particles is 95:5 to 70:
30.
4. The ABS composite material according to claim 1, characterized in that: The melt mass flow rate of the ABS resin is 5 to 10 g / 10 min.
5. The ABS composite material according to claim 1, characterized in that: At least one of the following conditions is also met: The lubricant comprises at least one of PETS, EBS, zinc stearate and montan acid wax; The inorganic filler includes wollastonite; The aspect ratio of the inorganic filler is 1 to 3; The solvent blue is solvent blue 104 , and the solvent red is solvent red 207 .
6. The ABS composite material according to any one of claims 1 to 5, characterized in that: The ABS composite material meets at least one of the following conditions: Glossiness is 35-50GU; Thermal deformation temperature is 80-90°C; Notch impact: 9~15KJ / m 2 ; The tensile strength is 46~65MPa.
7. A method for preparing the ABS composite material according to any one of claims 1 to 6, characterized in that: include: Mixing the first composition particles and the second composition particles in a predetermined ratio to obtain mixed particles; The mixed particles are injection molded to obtain the ABS composite material.
8. The method according to claim 7, characterized in that The preparation method of the first composition particles comprises: Stirring the raw materials of the first composition particles at high speed for first premixing to obtain a first mixture; The first mixture is added through the main feed port of a twin-screw extruder, and is subjected to first melt blending, cooling and granulation to obtain the first composition particles. The preparation method of the second composition particles comprises: Stirring the raw materials of the second composition particles at high speed for second premixing to obtain a second mixture; The second mixture is added into the main feeding port of the twin-screw extruder, and undergoes a second melt blending, cooling and granulation to obtain the second composition particles.
9. The method according to claim 8, characterized in that The mixing temperature of the first premixing and the second premixing is not higher than 60° C., the stirring speed is 800 to 1200 r / min, and the mixing time is 1 to 2 min; During the first melt blending process, the temperature is 190-230° C., and the screw speed of the twin-screw extruder is 500-600 r / min; During the second melt blending process, the temperature is 200-250° C., and the screw speed of the twin-screw extruder main machine is 500-600 r / min.
10. An appearance decoration, characterized in that: The ABS composite material comprises the ABS composite material according to any one of claims 1 to 6.