Resin composition and IC carrier tape

By covering a resin composition film containing flexible groups on the surface of the IC tape substrate, the problem of surface roughness of the substrate is solved, the toughness and electrical properties of the substrate are improved, and it is suitable for flexible packaging, so it is achieved. Accuracy chip packaging requirements.

CN119081351APending Publication Date: 2024-12-06广东伊帕思新材料科技有限公司
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411199196.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

During the production process, the existing IC tape carrier substrates are too rough due to the difference in yarn density of glass fiber fabrics and resin drift, which affects the chip bonding strength and electrical performance, especially when the chip size is reduced, the surfaces are more required. The roughness problem is difficult to solve.

Method used

Using a resin composition, including a base epoxy resin, MDI modified epoxy resin, tough resin, curing agent, accelerator, flame retardant, leveling agent and inorganic filler, the main chain of the MDI modified epoxy resin contains Multiple flexible groups, through specific component proportions and structural design, form a layer of adhesive film with a thickness of no more than 10 μm to cover the surface of the substrate, improving leveling performance and wettability to reduce surface roughness.

Benefits of technology

Effectively reduce the surface roughness difference between the weft and weft lines of the substrate surface, improve the toughness and electrical properties of the substrate, and is suitable for flexible packaging substrates, and significantly improves the substrate without affecting the performance of the IC tape. surface quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005017397050000021
    Figure BDA0005017397050000021
  • Figure BDA0005017397050000041
    Figure BDA0005017397050000041
  • Figure BDA0005017397050000051
    Figure BDA0005017397050000051
Patent Text Reader

Abstract

The invention discloses a resin composition which comprises the following components in parts by weight: 20-60 parts of basic epoxy resin, 1-10 parts of MDI modified epoxy resin, 1-20 parts of tough resin, 1-5 parts of a curing agent, 1-3 parts of an accelerant, 1-10 parts of a flame retardant, 1-5 parts of a flatting agent and 10-30 parts of inorganic filler, and the main chain of the MDI modified epoxy resin contains a plurality of flexible groups. The MDI modified epoxy resin is compounded with the basic epoxy resin and the tough resin in a specific proportion, so that the leveling performance and the wettability of the resin composition can be improved, good toughness is ensured, the roughness of the surface of a base material is effectively reduced, a main chain of the MDI modified epoxy resin contains a plurality of flexible groups, and the flexibility of the resin composition is improved. The main chain of the epoxy resin does not have excessive rigid groups and heterocyclic structures, but has a large number of flexible groups, so that the epoxy resin is very suitable for flexible packaging substrates, and the toughness of the epoxy resin is remarkably superior to that of epoxy resin with the main chain containing rigid groups or heterocyclic rings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor packaging technology, in particular to a resin composition and an IC carrier tape. Background Art

[0002] Smart cards are replacing magnetic cards in more and more fields due to their advantages of miniaturization, high reliability and low information loss. The production process of smart cards involves a packaging process, which is currently generally carried out using a high-efficiency roll-to-roll process. Therefore, the packaging carrier used to carry the chip is mostly made of flexible packaging substrate, that is, IC carrier substrate.

[0003] At present, IC carrier substrates are made by the traditional copper-clad laminate semi-cured sheet production process, that is, the glass fiber fabric is impregnated, baked, and post-cured to obtain the carrier substrate. However, due to the difference in yarn density between the warp and weft directions of the glass fiber fabric, and the existence of problems such as resin sag during the gluing process, the substrate produced by this process has a large surface roughness, especially the large difference in surface roughness between the warp and weft directions. The surface roughness of the substrate directly affects the bonding strength, electrical performance and reliability between the chip and the substrate. With the continuous development of technology, the chip size continues to decrease, and the surface roughness requirements of the carrier substrate are also getting higher and higher. Therefore, it is necessary to propose a new solution to solve the above problems. Summary of the invention

[0004] In view of this, the present invention aims to address the deficiencies in the prior art, and its main purpose is to provide a resin composition and an IC carrier, which can effectively solve the problem of large differences in surface roughness between the longitude and latitude lines on the surface of the substrate.

[0005] To achieve the above purpose, the present invention adopts the following technical solutions:

[0006] A resin composition comprises the following components in parts by weight: 20-60 parts of a basic epoxy resin, 1-10 parts of an MDI-modified epoxy resin, 1-20 parts of a toughening resin, 1-5 parts of a curing agent, 1-3 parts of an accelerator, 1-10 parts of a flame retardant, 1-5 parts of a leveling agent and 10-30 parts of an inorganic filler, wherein the main chain of the MDI-modified epoxy resin contains a plurality of flexible groups.

[0007] As a preferred solution, the main chain of the MDI modified epoxy resin also contains an ester group, and the molecular chain of the MDI modified epoxy resin contains a large amount of flexible matrix and ester group, which ensures the toughness of the coating and has good color performance, with little impact on the appearance of the material.

[0008] As a preferred embodiment, the flexible group is one or more of a methylene group, an ether bond and an amino group.

[0009] As a preferred embodiment, the structural formula of the MDI modified epoxy resin is

[0010]

[0011] As a preferred embodiment, the base epoxy resin is one or more of bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, hydrogenated bisphenol A epoxy resin, phenolic epoxy resin, alicyclic epoxy resin, and phosphorus-containing epoxy resin, preferably bisphenol F epoxy resin. Bisphenol F epoxy resin has methylene groups on the main chain of the molecule, has small steric hindrance, low resin viscosity, good wettability to glass fiber fabrics, and good leveling performance. The base epoxy resin is 40-50 parts.

[0012] As a preferred embodiment, the tough resin is one or more of phenolic resin, polyvinyl butyral resin, carboxyl liquid nitrile rubber, terminal carboxyl liquid nitrile rubber, core-shell rubber, and core-shell rubber modified epoxy resin, preferably terminal carboxyl liquid nitrile rubber. The terminal carboxyl liquid nitrile rubber has active carboxyl groups at both ends of its molecular chain and can react with the base epoxy resin to form a sea-island structure to enhance the toughness of the base resin. The tough resin is 5-20 parts.

[0013] As a preferred embodiment, the curing agent is one or more of an amine curing agent, an acid anhydride curing agent, a phenolic curing agent, and a styrene-maleic anhydride copolymer, preferably an aromatic diamine curing agent. The cured product formed after the aromatic diamine reacts with the epoxy resin has good heat resistance and mechanical properties, and the molar ratio of the curing agent to the base epoxy resin is 0.85-1.15.

[0014] As a preferred solution, the accelerator is an imidazole accelerator or a phenol accelerator, preferably an imidazole accelerator; the leveling agent is one or more of isophorone, diacetone alcohol, and an organosilicon leveling agent.

[0015] As a preferred embodiment, the flame retardant is at least one of DOPO and its derivatives, phosphazene flame retardants, nitrogen-based flame retardants, and inorganic flame retardants, preferably DOPO and its derivatives. The introduction of organic phosphorus compounds such as DOPO and its derivatives ensures good flame retardant properties. The flame retardant is 5-10 parts; the inorganic filler is one or more of silicon dioxide, aluminum hydroxide, magnesium hydroxide, aluminum oxide, boron nitride, talc, and silicon micropowder that have not been surface treated, and the particle size of the inorganic filler does not exceed 5μm.

[0016] An IC carrier tape comprises a substrate, on which a layer of adhesive film is coated. The thickness of the adhesive film does not exceed 10 μm, and the material of the adhesive film is the above-mentioned resin composition.

[0017] Compared with the prior art, the present invention has obvious advantages and beneficial effects. Specifically, it can be seen from the above technical solution that:

[0018] MDI-modified epoxy resin can be compounded with basic epoxy resin and toughening resin in a specific ratio to improve the leveling performance and wetting performance of the resin composition and ensure good toughness, thereby effectively reducing the roughness of the substrate surface. In addition, the main chain of MDI-modified epoxy resin contains multiple flexible groups. There are no excessive rigid groups and heterocyclic structures on the main chain, but there are a large number of flexible groups. It is very suitable for flexible packaging substrates, and its toughness is significantly better than that of epoxy resins containing rigid groups or heterocyclic rings in the main chain.

[0019] In order to more clearly illustrate the effects of the present invention, the present invention is described in detail below in conjunction with specific embodiments. DETAILED DESCRIPTION

[0020] The present invention discloses a resin composition, which comprises the following components by weight: 20-60 parts of a basic epoxy resin, 1-10 parts of an MDI-modified epoxy resin, 1-20 parts of a toughening resin, 1-5 parts of a curing agent, 1-3 parts of an accelerator, 1-10 parts of a flame retardant, 1-5 parts of a leveling agent and 10-30 parts of an inorganic filler, wherein the main chain of the MDI-modified epoxy resin contains a plurality of flexible groups.

[0021] The basic epoxy resin is one or more of bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, hydrogenated bisphenol A epoxy resin, phenolic epoxy resin, alicyclic epoxy resin, and phosphorus-containing epoxy resin, preferably bisphenol F epoxy resin. Bisphenol F epoxy resin has methylene on the main chain of the molecule, small steric hindrance, low resin viscosity, good wettability to glass fiber fabric, and good leveling performance. The basic epoxy resin is preferably 40-50 parts.

[0022] The main chain of the MDI modified epoxy resin also contains an ester group. The molecular chain of the MDI modified epoxy resin contains a large number of flexible matrices and ester groups, which ensures the toughness of the coating and has good color performance, and has little effect on the appearance of the material; and the flexible group is one or more of a methylene group, an ether bond and an amino group. Specifically, the structural formula of the MDI modified epoxy resin is

[0023] Specifically, the preparation method of the MDI modified epoxy resin is as follows:

[0024] 4,4′-methylenebis(phenyl isocyanate) and 3-(4-(2-(4-(oxirane-2-ylmethoxy)phenyl)propane-2-yl)phenoxy)propane-1,2-diol are mixed and a proper amount of solvent is added, wherein the molar ratio n(NCO):n(OH)=1:1.05, then stirred and heated to 110-130°C at a rate of 2-3°C / min, reacted for 4-6 hours, to obtain the MDI modified epoxy resin. The reaction process is as follows:

[0025]

[0026] The tough resin is one or more of phenolic resin, polyvinyl butyral resin, carboxyl liquid nitrile rubber, terminal carboxyl liquid nitrile rubber, core-shell rubber, and core-shell rubber modified epoxy resin, preferably terminal carboxyl liquid nitrile rubber. The terminal carboxyl liquid nitrile rubber has active carboxyl groups at both ends of its molecular chain and can react with the base epoxy resin to form a sea-island structure to enhance the toughness of the base resin. The tough resin is preferably 5-20 parts.

[0027] The curing agent is one or more of an amine curing agent, an acid anhydride curing agent, a phenolic curing agent, and a styrene-maleic anhydride copolymer, preferably an aromatic diamine curing agent. The cured product formed after the aromatic diamine reacts with the epoxy resin has good heat resistance and mechanical properties, and the molar ratio of the curing agent to the basic epoxy resin is 0.85-1.15; the accelerator is an imidazole accelerator or a phenolic accelerator, preferably an imidazole accelerator; the leveling agent is one or more of isophorone, diacetone alcohol, and an organic silicon leveling agent; the flame retardant is at least one of DOPO and its derivatives, phosphazene flame retardant, nitrogen flame retardant, and inorganic flame retardant, preferably DOPO and its derivatives. The introduction of organic phosphorus compounds such as DOPO and its derivatives ensures good flame retardant properties, and the flame retardant is 5-10 parts; the inorganic filler is one or more of silicon dioxide, aluminum hydroxide, magnesium hydroxide, aluminum oxide, boron nitride, talc, and silicon powder that have not been surface treated, and the particle size of the inorganic filler does not exceed 5μm.

[0028] The present invention also discloses an IC carrier, which includes a substrate, a layer of adhesive film coated on the substrate, the thickness of the adhesive film does not exceed 10 μm, and the material of the adhesive film is the aforementioned resin composition; the manufacturing process is as follows: first, weigh the above components by weight; then add each component to a solvent and stir it for more than 3 hours, and homogenize it for at least 1 hour to prepare an adhesive solution with a solid content of 35-45%, wherein the solvent is preferably a non-protonic polar solvent; then, the obtained adhesive solution is coated on the surface of the substrate to form an adhesive film, and the thickness of the adhesive film does not exceed 10 μm, and the coated substrate is placed in an oven at 120-200°C and baked for 3-10 minutes to obtain an IC carrier. The substrate comprises the following components: 25 parts of basic epoxy resin, 3 parts of tough resin, 2 parts of curing agent, 25 parts of inorganic filler, 2 parts of accelerator, 2 parts of coupling agent, and 5 parts of flame retardant.

[0029] In order to further illustrate the advantages of the present invention, a number of embodiments and comparative examples are listed for detailed description.

[0030] The raw materials used in the embodiments and comparative examples are shown in Table 1:

[0031] Table 1.

[0032] The component ratios of Examples 1-5 are shown in Table 2:

[0033]

[0034]

[0035] Table 2.

[0036] Comparative Examples 1 and 2 are both uncoated IC carrier substrates. The component ratio of Comparative Example 1 is consistent with the substrate selected in the embodiment, and the component ratio of Comparative Example 2 includes the following components: 25 parts of basic epoxy resin, 5 parts of toughening resin, 2 parts of curing agent, 25 parts of inorganic filler, 2 parts of accelerator, 2 parts of coupling agent, and 3 parts of leveling agent.

[0037] The performance tests of the above-mentioned multiple IC carriers are carried out in the following manner:

[0038] Glass transition temperature: Differential Scanning Calorimetry (DSC), heating rate 20°C / min.

[0039] Glue overflow: Take a 4-inch*4-inch sample and punch two circular holes with a diameter of 3 mm using a manual die punch. Stack the punched substrates according to IPC-TM-650 in the order of (steel plate / cushion material / release film / punched substrate / release film / cushion material / steel plate). Hot press for 10 minutes at a temperature of 171±3°C and a pressure of 200±10psi. After hot pressing, use an optical microscope to measure the glue flow at three positions with an interval of 120° and take the average value.

[0040] Surface energy: A water drop angle measuring instrument was used, the test liquids were water and diiodomethane, and the calculation method was the OWRK method.

[0041] Surface roughness: Use a surface roughness tester to test the Rz value, measure 25 sets of data at different locations and take the average value.

[0042] Dimensional stability: According to IPC-TM-650, the sample size is 300mm*280mm (warp*weft), and four circular holes with a diameter of 1.85mm are drilled in the four corners of the sample. The initial center distance of the four circular holes is measured by a two-dimensional measuring instrument with an accuracy of 0.001mm. After the test, the sample is placed in an oven at 150±5℃ and baked for 2h±5min. After the baking is completed, the center distance of the four circular holes is immediately tested after the sample cools to room temperature, and the dimensional change rate is calculated.

[0043] Flammability: UL94 vertical combustion method.

[0044] The test results are shown in Table 3.

[0045]

[0046] Table 3.

[0047] Analyzing the above data, comparing Comparative Example 1 with Comparative Example 2, no flame retardant was added to Comparative Example 2, so the flame retardancy of Comparative Example 2 was worse than that of Comparative Example 1. However, due to the addition of a leveling agent in Comparative Example 2, the surface leveling performance and wetting performance of the base layer were improved, thereby effectively reducing the roughness of the substrate surface, and the component ratio of the substrate can be changed, so that other properties of the substrate are changed.

[0048] Comparing Examples 1-5 with Comparative Example 2, the MDI-modified epoxy resin is compounded with the basic epoxy resin and the toughening resin in a specific ratio. Only 0.5 parts of the leveling agent are needed to significantly improve the roughness of the substrate, and the difference between the weft roughness and the warp roughness is much lower than that of Comparative Example 1 and Comparative Example 2. Moreover, the performance of the substrate is not affected by coating on the surface of the substrate to form a film.

[0049] At the same time, the MDI modified epoxy resin in the present invention contains structures such as methylene, ester and hydroxyl groups on the main chain, which helps to reduce the crystallinity, and the molecular chain is more likely to form a disordered arrangement. When used as a coating, it has better optical performance, no dark effect, and does not affect the appearance of the carrier substrate. At the same time, there are no excessive rigid groups and heterocyclic structures, but there are a large number of flexible groups such as methylene and ether bonds, which are very suitable for flexible packaging substrates. Its toughness is significantly better than that of epoxy resins containing rigid groups or heterocycles in the main chain.

[0050] In summary, the present invention covers the surface of the substrate with a very thin layer of adhesive film having excellent toughness, wettability and leveling properties. Compared with directly changing the substrate formula, the present invention can significantly reduce the surface roughness of the substrate, especially the surface roughness difference in the warp and weft directions, without affecting the performance of the IC carrier substrate.

[0051] The above description is only a preferred embodiment of the present invention and does not limit the technical scope of the present invention. Therefore, any slight modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A resin composition, characterized in that: The invention comprises the following components by weight: 20-60 parts of basic epoxy resin, 1-10 parts of MDI modified epoxy resin, 1-20 parts of toughening resin, 1-5 parts of curing agent, 1-3 parts of accelerator, 1-10 parts of flame retardant, 1-5 parts of leveling agent and 10-30 parts of inorganic filler, wherein the main chain of the MDI modified epoxy resin contains multiple flexible groups.

2. The resin composition according to claim 1, characterized in that: The main chain of the MDI modified epoxy resin also contains an ester group.

3. The resin composition according to claim 1, characterized in that: The flexible group is one or more of a methylene group, an ether bond and an amino group.

4. The resin composition according to claim 1, characterized in that: The structural formula of the MDI modified epoxy resin is 5. The resin composition according to claim 1, characterized in that: The basic epoxy resin is one or more of bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, hydrogenated bisphenol A epoxy resin, phenolic epoxy resin, alicyclic epoxy resin, phosphorus-containing epoxy resin, and the basic epoxy resin is 40-50 parts.

6. The resin composition according to claim 1, characterized in that: The tough resin is one or more of phenolic resin, polyvinyl butyral resin, carboxyl liquid nitrile rubber, carboxyl-terminated liquid nitrile rubber, core-shell rubber, and core-shell rubber modified epoxy resin, and the tough resin is 5-20 parts.

7. The resin composition according to claim 1, characterized in that: The curing agent is one or more of an amine curing agent, an acid anhydride curing agent, a phenol curing agent, and a styrene-maleic anhydride copolymer, and the molar ratio of the curing agent to the basic epoxy resin is 0.85-1.

15.

8. The resin composition according to claim 1, characterized in that: The accelerator is an imidazole accelerator or a phenol accelerator; the leveling agent is one or more of isophorone, diacetone alcohol, and an organosilicon leveling agent.

9. The resin composition according to claim 1, characterized in that: The flame retardant is at least one of DOPO and its derivatives, phosphazene flame retardants, nitrogen-based flame retardants, and inorganic flame retardants, and the flame retardant is 5-10 parts; the inorganic filler is one or more of silicon dioxide, aluminum hydroxide, magnesium hydroxide, aluminum oxide, boron nitride, talc, and silicon powder that have not been surface treated, and the particle size of the inorganic filler does not exceed 5μm.

10. An IC carrier tape, characterized in that: The invention comprises a substrate, on which a layer of adhesive film is coated, the thickness of the adhesive film does not exceed 10 μm, and the material of the adhesive film is the resin composition according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Adhesive with high glass transition temperature for flexible cover film

    CN105860896A

  • Low odor and high mold flow epoxy resin composition and application thereof

    CN108485186A

  • Glue solution composition, copper-clad plate and corresponding preparation method

    CN111073214A

  • Adhesive composition with high glass transition temperature and application thereof

    CN111234753A