PLA / PCL / rubber heat shrink film based on dynamic vulcanization technology and preparation method thereof
Through dynamic vulcanization technology combined with PLA, PCL and rubber, the problem of difficult degradation of heat shrink film materials and complex process is solved, and PLA/PCL/rubber film with high strength, high ductility and excellent heat shrinkage performance is achieved, which simplifies the process and Reduced costs.
Patent Information
- Application Number
- CN202411279787.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-12
AI Technical Summary
The existing heat shrink film materials are difficult to degrade, the manufacturing process is complex and the cost is high. The low molecular chain entanglement of commercial PLA resins leads to low melt strength and it is difficult to stably blow-molded film, limiting their application in the packaging market.
Using dynamic vulcanization technology, combined with PLA, PCL and rubber, dynamic vulcanization is carried out through peroxide as crosslinking agent to prepare PLA/PCL/rubber TPV blown film masterbatch. PCL and rubber are used to improve the brittleness of PLA and improve interface compatibility. and mechanical properties to achieve high strength, high ductility and excellent thermal shrinkage performance.
The tear strength, elongation of break and heat shrinkage of PLA/PCL/rubber films are significantly improved, the film blowing process is simplified, the production cost is reduced, and the efficient heat shrinkage function is achieved.
Smart Images

Figure CN119081372A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of PLA composite film preparation, and particularly relates to a PLA / PCL / rubber heat shrinkable film based on dynamic vulcanization technology and a preparation method thereof. Background Art
[0002] There are many types of plastic packaging films, among which the market demand for heat shrinkable films is growing at an alarming rate, becoming a hot spot in the plastic packaging industry. Heat shrinkable film is a polymer shape memory film that uses the changes in the fixed phase and reversible phase inside the polymer to achieve film shrinkage. Currently, commonly used heat shrinkable films include PVC, PE, PP, PVDC, OPS, PET, etc., but the heat shrinkable films made of these materials are difficult to degrade, which is very harmful to the environment and does not conform to the concept of green and environmentally friendly development. In addition, these heat shrinkable films usually adopt unidirectional and bidirectional stretching methods, and the manufacturing process is complicated and costly. Therefore, the industry urgently needs to develop a new type of heat shrinkable film material that is both degradable and easy to process.
[0003] The biodegradability of polylactic acid (PLA) gives it great potential for application in many fields, especially in the field of packaging materials. In the production of packaging materials, blown film technology is popular because of its high production efficiency and ability to produce polymer films with excellent macroscopic properties. However, unmodified commercial PLA resin has low molecular chain entanglement, which makes its melt strength quite low, making it difficult to stably blown into film. In addition, the brittleness of PLA further limits its practicality in the plastics market. It is precisely because of these problems that PLA has not yet been able to replace petroleum-based polymers such as low-density polyethylene (LDPE) that are currently widely used in the blown film process.
[0004] Chinese patent CN115891367A discloses a PBAT-PLA composite material and its application in a biodegradable heat shrinkable film, wherein the PBAT-PLA composite material is prepared by three-layer co-extrusion blow molding with PBAT as the inner and outer layers and PLA cross-linked PBAT as the middle layer, and the biodegradable heat shrinkable film prepared by the blow molding process has excellent tensile properties and impact resistance, etc. However, the invention is to prepare a film with heat shrinkability by three-layer co-extrusion blow molding, and the production process is cumbersome and the cost is high. Summary of the invention
[0005] In order to overcome the deficiencies of the prior art, the object of the present invention is to provide a PLA / PCL / rubber heat shrinkable film based on dynamic vulcanization technology and a preparation method thereof, wherein the film has high strength, high ductility, and excellent heat shrinkage performance.
[0006] To achieve the above object, the technical solution adopted by the present invention is:
[0007] A PLA / PCL / rubber heat shrinkable film based on dynamic vulcanization technology and a preparation method thereof. The raw material ratio composition is as follows, by weight: 60-80 parts of polylactic acid, 10-20 parts of polycaprolactone, 3-20 parts of rubber, 0.2-2 parts of antioxidant, and 0.015-0.6 parts of cross-linking agent.
[0008] Furthermore, the polylactic acid is one or more of poly-L-lactic acid, poly-D-lactic acid and racemic polylactic acid.
[0009] Furthermore, the rubber is one or more of natural rubber, epoxy natural rubber, and nitrile rubber.
[0010] Furthermore, the amount of the antioxidant is 0.2%-2% of the total mass of the rubber and plastic, and the antioxidant is one or more of antioxidant 168, antioxidant 1076, antioxidant 1010, antioxidant CA, antioxidant B900, antioxidant BHT, antioxidant 264, and antioxidant DLTP.
[0011] Furthermore, the crosslinking agent is a peroxide, and the amount of the peroxide is 0.5%-3% of the rubber mass; the peroxide is one or more of dicumyl peroxide, benzoyl peroxide, di-tert-butyl peroxide and tert-butyl perbenzoate.
[0012] A method for preparing a PLA / PCL / rubber heat shrinkable film based on dynamic vulcanization technology comprises the following steps:
[0013] Step 1: First, mix polycaprolactone, rubber, cross-linking agent and antioxidant in an internal mixer and then crush them into small particles.
[0014] Step 2: melt-blending the blend obtained in step 1 with PLA in a twin-screw according to a certain ratio, extruding and granulating to obtain a blown film masterbatch.
[0015] Step 3: Add the film blowing masterbatch obtained in step 2 into a single-screw film blowing machine, and blow mold to obtain an ultra-tough PLA / PCL / rubber bio-based degradable film with heat shrinkage performance.
[0016] In the above method, in step 1, the temperature of the internal mixer is 60-110° C., and the blending time is about 3-10 min.
[0017] In the above method, in step 2, the temperature of the twin-screw extruder is 150° C.-190° C., and the screw speed is 50-400 r / min.
[0018] In the above method, in step 2, PLA, PCL and rubber are sheared and vulcanized under the action of a cross-linking agent to prepare a PLA / PCL / rubber TPV blown film masterbatch through dynamic vulcanization.
[0019] In the above method, in step 3, the temperature of the single screw film blowing machine is 150°C-180°C, and the screw speed is 50-400r / min.
[0020] Compared with the prior art, the present invention has the following advantages:
[0021] 1) The present invention uses PCL and rubber as toughening agents for PLA. Under the synergistic effect of PCL and rubber, the brittleness of PLA can be effectively improved, so that the PLA / PCL / rubber film has excellent tear strength and elongation at break.
[0022] 2) For blends, the compatibility between different phases will directly affect the performance of the material. The present invention uses peroxide as a crosslinking agent and adopts a dynamic vulcanization method to prepare PLA / PCL / rubber TPV blown film masterbatch. Peroxide not only decomposes to produce free radicals to initiate rubber crosslinking, but also can trigger a grafting reaction between plastic and rubber, significantly improving the interfacial compatibility between the plastic phase and the rubber phase, so that the material has better mechanical properties.
[0023] 4) The PLA / PCL / rubber TPV material obtained by dynamic vulcanization in the present invention has a co-continuous phase structure, which can significantly improve the melt strength of the material and make the blow molding film forming process more stable and efficient.
[0024] 5) The PLA / PCL / rubber TPV material obtained by dynamic vulcanization in the present invention has a co-continuous phase structure, that is, PLA and cross-linked rubber are both continuous phase structures, and the film obtained after the blow molding process is still a co-continuous phase structure, and an excellent heat shrinkage function can be achieved through a simple film blowing process, thereby avoiding the need for conventional heat shrinkable films to undergo complex unidirectional and bidirectional stretching processes. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a scanning electron microscope image of the PLA / PCL / rubber TPV blown film masterbatch in Example 4 after being etched with dichloromethane.
[0026] Figure 2 This is a scanning electron microscope image of the surface of the PLA / PCL / rubber film obtained in Example 4 after being etched with dichloromethane. DETAILED DESCRIPTION
[0027] The technical scheme in the embodiments of the present invention will be described clearly and completely below in combination with the embodiments of the present invention and the accompanying drawings. However, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. PLA and PCL in the embodiments and the comparative examples were dried in a drying oven at 60°C for 8 hours before use, and the rubber was plasticized on an open mill before use.
[0028] The raw materials and sources of the following reference examples and embodiments:
[0029] Polylactic acid was selected as the matrix resin (REVODE110, Zhejiang Hisun Biomaterials Co., Ltd.). PCL (Capa6800) was purchased from Solvay, USA. The rubber used was natural rubber purchased from Guangzhou Rubber Industry Research Institute. The crosslinking agent used was DCP, and the antioxidant was antioxidant 1010.
[0030] Comparative Example 1
[0031] 20 parts of PCL were added into a torque rheometer at a temperature of 70°C and a rotor speed of 60 r / min, and after melting, antioxidant 1010 (0.2 parts) was added, and after mixing evenly, the PCL blend was obtained. The sample was crushed into fine particles using a crusher.
[0032] The PCL blend obtained in the above steps was mixed with 80 parts of PLA and then added to a twin-screw extruder for melt plasticization, blending, extrusion granulation to obtain PLA / PCL film blowing masterbatch. The parameters of the twin-screw extruder are: the temperature of zone 1 is 130-160°C, the temperature of zone 2 is 170-180°C, the temperature of zone 3 is 180-190°C, the temperature of zone 4 is 180-185°C, and the head temperature is 180°C. The screw speed is 150rpm.
[0033] The film blowing masterbatch was blown into film by a single screw film blowing machine to obtain a PLA / PCL blown film. The temperature of the single screw film blowing machine was 165°C-175°C, and the head temperature was 170°C.
[0034] Comparative Example 2
[0035] 20 parts of PCL and 15 parts of natural rubber were added to a torque rheometer at a temperature of 70°C and a rotor speed of 60 r / min, and after being mixed evenly, antioxidant 1010 (0.23 parts) was added, and after being mixed evenly, a PCL / natural rubber blend was obtained. The blend was crushed into fine particles using a crusher.
[0036] The PCL / natural rubber blend obtained in the above steps was mixed with 80 parts of PLA and then added to a twin-screw extruder for melt plasticization, blending, extrusion granulation to obtain PLA / PCL / natural rubber blown film masterbatch. The parameters of the twin-screw extruder are: the temperature of zone 1 is 130-160°C, the temperature of zone 2 is 170-180°C, the temperature of zone 3 is 180-190°C, the temperature of zone 4 is 180-185°C, and the head temperature is 180°C. The screw speed is 150rpm.
[0037] The film blowing masterbatch is blown into film by a single-screw film blowing machine to obtain a PLA / PCL / rubber heat shrinkable film based on dynamic vulcanization technology and a preparation method thereof. The temperature of the single-screw film blowing machine is 165°C-175°C, and the head temperature is 170°C.
[0038] Example 1
[0039] 20 parts of PCL and 3 parts of natural rubber were added to a torque rheometer at a temperature of 70°C and a rotor speed of 60 r / min. After being mixed evenly, antioxidant 1010 (0.206 parts) and crosslinking agent DCP (0.045 parts) were added. After being mixed evenly, the PCL / natural rubber blend was obtained. The blend was crushed into fine particles using a crusher.
[0040] The PCL / natural rubber blend obtained in the above steps was mixed with 80 parts of PLA and then added to a twin-screw extruder for melt plasticization, blending, dynamic vulcanization, and extrusion granulation to obtain PLA / PCL / natural rubber blown film masterbatch. The parameters of the twin-screw extruder are: the temperature of zone 1 is 130-160°C, the temperature of zone 2 is 170-180°C, the temperature of zone 3 is 180-190°C, the temperature of zone 4 is 180-185°C, and the head temperature is 180°C. The screw speed is 150rpm.
[0041] The film blowing masterbatch is blown into film by a single-screw film blowing machine to obtain a PLA / PCL / rubber heat shrinkable film based on dynamic vulcanization technology and a preparation method thereof. The temperature of the single-screw film blowing machine is 165°C-175°C, and the head temperature is 170°C.
[0042] Example 2
[0043] 20 parts of PCL and 5 parts of natural rubber were added to a torque rheometer at a temperature of 70°C and a rotor speed of 60 r / min. After being mixed evenly, antioxidant 1010 (0.210 parts) and crosslinking agent DCP (0.075 parts) were added. After being mixed evenly, the PCL / natural rubber blend was obtained. The blend was crushed into fine particles using a crusher.
[0044] The PCL / natural rubber blend obtained in the above steps was mixed with 80 parts of PLA and then added to a twin-screw extruder for melt plasticization, blending, dynamic vulcanization, and extrusion granulation to obtain PLA / PCL / natural rubber blown film masterbatch. The parameters of the twin-screw extruder are: the temperature of zone 1 is 130-160°C, the temperature of zone 2 is 170-180°C, the temperature of zone 3 is 180-190°C, the temperature of zone 4 is 180-185°C, and the head temperature is 180°C. The screw speed is 150rpm.
[0045] The film blowing masterbatch is blown into film by a single-screw film blowing machine to obtain a PLA / PCL / rubber heat shrinkable film based on dynamic vulcanization technology and a preparation method thereof. The temperature of the single-screw film blowing machine is 165°C-175°C, and the head temperature is 170°C.
[0046] Example 3
[0047] 20 parts of PCL and 7 parts of natural rubber were added to a torque rheometer at a temperature of 70°C and a rotor speed of 60 r / min. After being mixed evenly, antioxidant 1010 (0.214 parts) and crosslinking agent DCP (0.105 parts) were added. After being mixed evenly, the PCL / natural rubber blend was obtained. The blend was crushed into fine particles using a crusher.
[0048] The PCL / natural rubber blend obtained in the above steps was mixed with 80 parts of PLA and then added to a twin-screw extruder for melt plasticization, blending, dynamic vulcanization, and extrusion granulation to obtain PLA / PCL / natural rubber blown film masterbatch. The parameters of the twin-screw extruder are: the temperature of zone 1 is 130-160°C, the temperature of zone 2 is 170-180°C, the temperature of zone 3 is 180-190°C, the temperature of zone 4 is 180-185°C, and the head temperature is 180°C. The screw speed is 150rpm.
[0049] The film blowing masterbatch is blown into film by a single-screw film blowing machine to obtain a PLA / PCL / rubber heat shrinkable film based on dynamic vulcanization technology and a preparation method thereof. The temperature of the single-screw film blowing machine is 165°C-175°C, and the head temperature is 170°C.
[0050] Example 4
[0051] 20 parts of PCL and 10 parts of natural rubber were added to a torque rheometer at a temperature of 70°C and a rotor speed of 60 r / min. After being mixed evenly, antioxidant 1010 (0.220 parts) and crosslinking agent DCP (0.15 parts) were added. After being mixed evenly, the PCL / natural rubber blend was obtained. The blend was crushed into fine particles using a crusher.
[0052] The PCL / natural rubber blend obtained in the above steps was mixed with 80 parts of PLA and then added to a twin-screw extruder for melt plasticization, blending, dynamic vulcanization, and extrusion granulation to obtain PLA / PCL / natural rubber blown film masterbatch. The parameters of the twin-screw extruder are: the temperature of zone 1 is 130-160°C, the temperature of zone 2 is 170-180°C, the temperature of zone 3 is 180-190°C, the temperature of zone 4 is 180-185°C, and the head temperature is 180°C. The screw speed is 150rpm.
[0053] The film blowing masterbatch is blown into film by a single-screw film blowing machine to obtain a PLA / PCL / rubber heat shrinkable film based on dynamic vulcanization technology and a preparation method thereof. The temperature of the single-screw film blowing machine is 165°C-175°C, and the head temperature is 170°C.
[0054] Example 5
[0055] 20 parts of PCL and 15 parts of natural rubber were added to a torque rheometer at a temperature of 70°C and a rotor speed of 60 r / min. After being mixed evenly, antioxidant 1010 (0.23 parts) and crosslinking agent DCP (0.225 parts) were added. After being mixed evenly, the PCL / natural rubber blend was obtained. The blend was crushed into fine particles using a crusher.
[0056] The PCL / natural rubber blend obtained in the above steps was mixed with 80 parts of PLA and then added to a twin-screw extruder for melt plasticization, blending, dynamic vulcanization, and extrusion granulation to obtain PLA / PCL / natural rubber blown film masterbatch. The parameters of the twin-screw extruder are: the temperature of zone 1 is 130-160°C, the temperature of zone 2 is 170-180°C, the temperature of zone 3 is 180-190°C, the temperature of zone 4 is 180-185°C, and the head temperature is 180°C. The screw speed is 150rpm.
[0057] The film blowing masterbatch is blown into film by a single-screw film blowing machine to obtain a PLA / PCL / rubber heat shrinkable film based on dynamic vulcanization technology and a preparation method thereof. The temperature of the single-screw film blowing machine is 165°C-175°C, and the head temperature is 170°C.
[0058] The properties of the control example and the embodiment are shown in Table 1.
[0059] The tensile test is based on GB / T1040-2006 standard.
[0060] The calculation of thermal shrinkage is as follows:
[0061]
[0062] Where L0 is the length of the sample before shrinkage, and L is the length of the sample after shrinkage.
[0063] Table 1
[0064]
[0065] As can be seen from Table 1, the addition of rubber can significantly improve the elongation at break of the film, but it will also reduce the tensile strength of the film. As the amount of rubber gradually increases, the thermal shrinkage of the film is significantly improved. This is because the addition of rubber allows the film to form a cross-linked three-dimensional network structure, which provides a strong recovery force for the film, which makes the film have excellent thermal shrinkage properties. The thermal shrinkage of Example 5 with the addition of 15 parts of rubber reached more than 35% in both the transverse and longitudinal directions. Compared with the film in Control Example 1 without the addition of rubber, the thermal shrinkage performance is improved by about 12.5 times. It can be seen from the comparison between Control Example 2 and Example 5 that dynamic vulcanization technology can significantly improve the thermal shrinkage of the film, because the cross-linked rubber network has a stronger shrinkage recovery force.
[0066] Figure 1 This is a scanning electron microscope image of the PLA / PCL / rubber TPV blown film masterbatch after being etched with dichloromethane in Example 4. Since both PLA and PCL are etched by dichloromethane, the network structure observed in the SEM image is a rubber cross-linked network structure.
[0067] Figure 2 This is a scanning electron microscope image of the surface of the PLA / PCL / rubber film obtained in Example 4 after being etched with dichloromethane. It can be seen from the figure that the rubber phase in the film still presents a three-dimensional network structure. Therefore, during the blow molding process, the dual continuous phase in the PLA / PCL / rubber material is not destroyed.
Claims
1. A PLA / PCL / rubber heat shrinkable film based on dynamic vulcanization technology, characterized in that: The raw material ratio is as follows, by weight: 60-80 parts of polylactic acid, 10-20 parts of polycaprolactone, 3-20 parts of rubber, 0.2-2 parts of antioxidant and 0.015-0.6 parts of cross-linking agent.
2. The PLA / PCL / rubber heat shrinkable film based on dynamic vulcanization technology according to claim 1, characterized in that: The polylactic acid is one or more of poly L-lactic acid, poly D-lactic acid and racemic polylactic acid.
3. The PLA / PCL / rubber heat shrinkable film based on dynamic vulcanization technology according to claim 1, characterized in that: The rubber is one or more of natural rubber, epoxy natural rubber, and nitrile rubber.
4. The PLA / PCL / rubber heat shrinkable film based on dynamic vulcanization technology according to claim 1, characterized in that: The antioxidant is one or more of antioxidant 168, antioxidant 1076, antioxidant 1010, antioxidant CA, antioxidant B900, antioxidant BHT, antioxidant 264, and antioxidant DLTP.
5. The PLA / PCL / rubber heat shrinkable film based on dynamic vulcanization technology according to claim 1, characterized in that: The crosslinking agent is a peroxide; the peroxide is one or more of dicumyl peroxide, di-tert-butyl diisopropyl peroxide, benzoyl peroxide, di-tert-butyl peroxide and tert-butyl perbenzoate.
6. A method for preparing a PLA / PCL / rubber heat shrinkable film based on dynamic vulcanization technology according to any one of claims 1 to 5, characterized in that: The following steps are involved: Step 1: Mix polycaprolactone, rubber, crosslinking agent and antioxidant in an internal mixer and crush them into granules; Step 2: melt blending the blend obtained in step 1 with PLA in a twin-screw extruder, dynamically vulcanizing, and extruding granulation to obtain PLA / PCL / rubber TPV film blowing masterbatch; Step 3: Add the PLA / PCL / rubber TPV film blowing masterbatch obtained in step 2 into a single-screw film blowing machine, and obtain a PLA / PCL / rubber bio-based film with heat shrinkage properties by film blowing.
7. A method for preparing a PLA / PCL / rubber heat shrinkable film based on dynamic vulcanization technology according to claim 6, characterized in that: In step 1, the temperature of the internal mixer is 60-110° C., and the blending time is about 3-10 min.
8. A method for preparing a PLA / PCL / rubber heat shrinkable film based on dynamic vulcanization technology according to claim 6, characterized in that: In step 2, the twin-screw extrusion temperature is 150°C-190°C, and the screw speed is 50-400r / min.
9. A method for preparing a PLA / PCL / rubber heat shrinkable film based on dynamic vulcanization technology according to claim 6, characterized in that: In step 2, PLA, PCL and rubber are sheared and vulcanized under the action of a cross-linking agent, and a PLA / PCL / rubber TPV blown film masterbatch is prepared by dynamic vulcanization.
10. A method for preparing a PLA / PCL / rubber heat shrinkable film based on dynamic vulcanization technology according to claim 6, characterized in that: In step three, the temperature of the single screw film blowing machine is 150°C-180°C, and the screw speed is 50-400r / min.
Citation Information
Patent Citations
Transparent high-toughness biaxially oriented polylactic acid film and preparation method thereof
CN114736497A
Preparation method and application of heat-resistant high-fluidity polylactic acid
CN115012058A
Biodegradable transparent heat shrinkage film material, preparation method and application
CN117362960A
Heat-shrinkable polylactic acid film
JP2003103632A
Diaphragm applicable to sound production device, preparation method thereof, and sound production device
WO2022262559A1
Cited By
TPE / rubber double-color master batch preparation method based on dynamic vulcanization technology
CN121718039A