Coffee residue composite decorative plate and preparation process thereof
By using coffee ground mixture in coffee ground composite decorative panels, the combination of materials such as nanosilane modified magnesium borate whisker-reinforced modified bamboo fibers and other materials, the problems of low utilization rate of coffee grounds and poor performance of the board in the prior art are solved. , realizes high-performance decorative panel preparation, suitable for high-performance areas.
Patent Information
- Application Number
- CN202411437348.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-15
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing coffee ground reuse technology has problems such as insufficient economics, limited practicality and insufficient performance, which is difficult to promote and apply in large-scale industrial production, especially in areas with high performance requirements.
The combination of coffee ground mixture and nanosilane modified magnesium borate whisker-reinforced modified bamboo fibers, phenolic resins and other materials is used to form a coffee ground composite decorative board through a specific preparation process to improve the mechanical strength, heat resistance and resistance of the board. Impact and flame retardant properties.
It significantly improves the environmental protection performance, mechanical properties and functionality of decorative panels, realizes the resource utilization of waste, is suitable for high-performance applications, and has broad market prospects and application value.
Smart Images

Figure BDA0005085404110000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite materials, and in particular to a coffee grounds composite decorative board and a preparation process thereof. Background Art
[0002] Coffee is the second most traded commodity in the world after oil, with nearly 10 million tons of raw coffee beans produced each year. After coffee beans are steamed, more than 90% of their dry matter is a byproduct of the process - coffee grounds. Coffee grounds are rich in a variety of polysaccharides, such as lignin, cellulose, hemicellulose, etc., and have a high utilization value.
[0003] According to statistics from relevant departments, my country currently produces about 730,000 tons of coffee grounds each year. However, the current methods for recycling coffee grounds are mainly concentrated in the following aspects: (1) Direct composting: Using coffee grounds as organic fertilizer directly on farmland is a relatively simple way of recycling. However, this method is limited to low-value-added applications and fails to fully tap the potential value of coffee grounds. (2) Adsorption and filling modification technology: This type of technology is mainly used to improve the physical properties of materials, such as enhancing the strength of materials by adsorbing heavy metal ions or acting as a filler. However, the application scope of these technologies is limited and there are still some limitations in actual operation. (3) Preparation of activated carbon: Although the method of preparing activated carbon from coffee grounds can increase the added value of coffee grounds, its preparation process is complicated, the cost is high, and the amount of coffee grounds used is not high, so it is difficult to promote and apply on a large scale. In summary, although the existing coffee grounds recycling technology has solved the problem of coffee grounds treatment to a certain extent, it still has limitations such as insufficient economy, limited practicality and limited practicality. Most technologies have high costs, making them difficult to promote and apply in large-scale industrial production, and some technologies have a narrow application scope and cannot meet a wider range of application needs. There are also some methods that produce products that have deficiencies in strength, durability, etc., which limits their application in fields requiring high performance.
[0004] Therefore, there is an urgent need for a coffee grounds composite decorative board and its preparation process to achieve high added value utilization and excellent performance of coffee grounds, so that it is suitable for applications requiring high heat resistance, mechanical strength, impact resistance and flame retardancy, and has broad market prospects and application value. Summary of the invention
[0005] To this end, the present invention provides a coffee grounds composite decorative board and a preparation process thereof, so as to solve the problems of low coffee grounds utilization and poor board performance in the prior art.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] According to a first aspect of the present invention, there is provided a coffee grounds composite decorative board, comprising the following components in parts by weight:
[0008] 200-500 parts of coffee grounds mixture, 13-30 parts of nano-silane modified magnesium borate whisker reinforced modified bamboo fiber, 15-35 parts of phenolic resin, 10-20 parts of sodium hydroxide, 600-900 parts of calcium silicate, 120-240 parts of diatomaceous earth powder, 12-36 parts of hollow microspheres, 15-25 parts of wollastonite, 1-3 parts of water retaining agent, 0.5-2 parts of polypropylene fiber, 6-12 parts of mildewproof agent, 32-46 parts of redispersible latex powder, 1-5 parts of nano zinc powder and 20-40 parts of water;
[0009] The coffee grounds mixture is formed by mixing coffee grounds, cork particles and polyurethane adhesive, wherein the mass ratio of the coffee grounds to the cork particles is (80-90):(10-20); the mass ratio of the polyurethane adhesive to the mixture of coffee grounds and cork particles is (80-120):(20-40).
[0010] Furthermore, the preparation method of the nano-silane modified magnesium borate whisker reinforced modified bamboo fiber comprises the following steps:
[0011] S1. Bamboo fiber pretreatment: The bamboo fiber is immersed in a hydrogen peroxide solution, impregnated to remove impurities, and then placed in a blast drying oven for drying to obtain alkaline hydrogen peroxide pretreated bamboo fiber;
[0012] S2. Modified magnesium borate whiskers: Nano magnesium borate whiskers and silane coupling agent are dispersed in dioxane, ultrasonically dispersed, and then heated to reflux at 100-110°C for 0.5-1.5h, then centrifuged to separate the precipitate, washed with anhydrous ethanol, and finally dried to obtain nano silane coupling agent modified magnesium borate whiskers;
[0013] S3. The alkaline hydrogen peroxide pretreated bamboo fiber is placed into the nano-silane coupling agent modified magnesium borate whisker, and then placed into a ball mill to remove the spheres and mixed evenly. The obtained bamboo fiber is placed in a vacuum drying oven and dried at 135-145° C. for 12-15 hours to obtain nano-silane modified magnesium borate whisker reinforced modified bamboo fiber.
[0014] Furthermore, in S1, the bamboo fiber is 25-40 parts by weight, the hydrogen peroxide solution is 800-1200 mL, and the mass fraction of the hydrogen peroxide solution is 1-3%.
[0015] Furthermore, in S1, after the bamboo fiber is immersed in the hydrogen peroxide solution, sodium hydroxide is gradually added to the mixed solution until the pH value is adjusted to 12-13.
[0016] Further, in said S1, the immersion temperature is 25-35°C, and the immersion time is 2-4h;
[0017] The drying temperature in the blast drying oven is 70-110° C., and the drying time is 8-12 hours.
[0018] Furthermore, the silane coupling agent in S2 is one or more of γ-glycidyloxypropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-chloropropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, and 3-isocyanatepropyltriethoxysilane.
[0019] Furthermore, in the S2, the nano-magnesium borate whisker is 4-7 parts by weight, the silane coupling agent is 9-16 parts by weight, and the dioxane is 80-100 parts by weight.
[0020] Furthermore, in S2, the ultrasonic dispersion time is 10-30 min; the heating reflux temperature is 90-110° C., the time is 0.5-2.5 h; the centrifugal speed is 5000-10000 rpm, and the centrifugal time is 5-15 min.
[0021] Furthermore, in S2, the separated precipitate is washed with anhydrous ethanol for 3-5 times, and the washed precipitate is placed in a vacuum drying oven and dried at 135-145° C. for 12-15 hours.
[0022] According to a second aspect of the present invention, a process for preparing the coffee grounds composite decorative board is provided, comprising the following steps:
[0023] S1. Weigh the raw materials prepared and add them to a high shear mixer and mix for 15-30min to obtain a primary mixture for later use;
[0024] S2. Pour the mixed material into a Z-type reamer mixer, stir and mix again for 10-20 minutes, then discharge and seal with polyester film to form a mass for storage;
[0025] S3. Heat the mold, then put the mass on the mold, use a 400T press to press, the pressing temperature is controlled at 130-150°C, and the finished product is demoulded and taken out after pressing for 13-17 minutes;
[0026] S4. Use a trimming machine to trim the decorative panels to the required specifications, and conduct quality inspection on the trimmed panels. After passing the inspection, they will be put into storage for future use.
[0027] The present invention has the following advantages:
[0028] 1. This application achieves significant improvements in the environmental performance, mechanical properties and functionality of the decorative board by adding a coffee grounds mixture, wherein the cork particles of different sizes added to the coffee grounds mixture increase the aesthetics of the board; the polyurethane adhesive added to the coffee grounds mixture increases the toughness of the decorative board. As one of the main ingredients, the coffee grounds mixture not only realizes the resource utilization of waste, but also improves the toughness and elasticity of the board, enhances its impact resistance, and its unique porous structure also gives the board excellent sound absorption and heat preservation properties.
[0029] 2. This application significantly improves the mechanical strength and toughness of the composite decorative board by using nano-silane modified magnesium borate whiskers to reinforce modified bamboo fibers, making it less likely to be damaged when subjected to external forces and having better impact resistance. The nano-silane coupling agent enhances the interfacial bonding between the bamboo fiber and the matrix material, improving the overall mechanical properties. The addition of nano-silane modified magnesium borate whiskers not only increases the thermal deformation temperature of the board, but also improves its flame retardant properties, which means that the board is less likely to deform in a high temperature environment and can provide higher safety in a fire.
[0030] 3. Through precise formula design and reasonable process flow, the performance of the board in many aspects has been optimized. The coffee grounds composite decorative board prepared by the technical solution of this application has excellent performance in terms of heat deformation temperature, tensile strength, notched impact strength and oxygen index. It is suitable for applications requiring high heat resistance, mechanical strength, impact resistance and flame retardancy, and has broad market prospects and application value. DETAILED DESCRIPTION
[0031] The following is a description of the implementation of the present invention by specific embodiments. People familiar with the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] The present invention provides a coffee grounds composite decorative board, comprising the following components in parts by weight:
[0033] 200-500 parts of coffee grounds mixture, 13-30 parts of nano-silane modified magnesium borate whisker reinforced modified bamboo fiber, 15-35 parts of phenolic resin, 10-20 parts of sodium hydroxide, 600-900 parts of calcium silicate, 120-240 parts of diatomaceous earth powder, 12-36 parts of hollow microspheres, 15-25 parts of wollastonite, 1-3 parts of water retaining agent, 0.5-2 parts of polypropylene fiber, 6-12 parts of mildewproof agent, 32-46 parts of redispersible latex powder, 1-5 parts of nano zinc powder and 20-40 parts of water;
[0034] The coffee grounds mixture is made of coffee grounds, cork particles and polyurethane adhesive, and the mass ratio of the coffee grounds to the cork particles is (80-90):(10-20); the mass ratio of the polyurethane adhesive to the mixture of coffee grounds and cork particles is (80-120):(20-40).
[0035] Specifically, the preparation method of nano-silane modified magnesium borate whisker reinforced modified bamboo fiber comprises the following steps:
[0036] S1. Bamboo fiber pretreatment: The bamboo fiber is immersed in a hydrogen peroxide solution, impregnated to remove impurities, and then placed in a blast drying oven for drying to obtain alkaline hydrogen peroxide pretreated bamboo fiber;
[0037] S2. Modified magnesium borate whiskers: Nano magnesium borate whiskers and silane coupling agent are dispersed in dioxane, ultrasonically dispersed, and then heated to reflux at 100-110°C for 0.5-1.5h, then centrifuged to separate the precipitate, washed with anhydrous ethanol, and finally dried to obtain nano silane coupling agent modified magnesium borate whiskers;
[0038] S3. The alkaline hydrogen peroxide pretreated bamboo fiber is placed into the nano-silane coupling agent modified magnesium borate whisker, and then placed into a ball mill to remove the spheres and mixed evenly. The obtained bamboo fiber is placed in a vacuum drying oven and dried at 135-145° C. for 12-15 hours to obtain nano-silane modified magnesium borate whisker reinforced modified bamboo fiber.
[0039] Specifically, in S1, the bamboo fiber is 25-40 parts by weight, the hydrogen peroxide solution is 800-1200 mL, and the mass fraction of the hydrogen peroxide solution is 1-3%.
[0040] Specifically, in S1, after the bamboo fiber is immersed in the hydrogen peroxide solution, sodium hydroxide is gradually added to the mixed solution until the pH value is adjusted to 12-13.
[0041] Specifically, in S1, the immersion temperature is 25-35°C, and the immersion time is 2-4h;
[0042] The drying temperature in the blast drying oven is 70-110°C and the drying time is 8-12h.
[0043] Specifically, the silane coupling agent in S2 is one or more of γ-glycidyloxypropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-chloropropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, and 3-isocyanatepropyltriethoxysilane. Preferably, the present application uses 3-isocyanatepropyltriethoxysilane.
[0044] Specifically, in S2, the nano magnesium borate whisker is 4-7 parts by weight, the silane coupling agent is 9-16 parts by weight, and the dioxane is 80-100 parts by weight.
[0045] Specifically, in S2, the ultrasonic dispersion time is 10-30 min; the heating reflux temperature is 90-110° C., the time is 0.5-2.5 h; the centrifugal speed is 5000-10000 rpm, and the centrifugal time is 5-15 min.
[0046] Specifically, in S2, the separated precipitate is washed with anhydrous ethanol for 3-5 times, and the washed precipitate is placed in a vacuum drying oven and dried at 135-145° C. for 12-15 hours.
[0047] The present invention provides a preparation process of the coffee grounds composite decorative board, comprising the following steps:
[0048] S1. Weigh the raw materials prepared and add them to a high shear mixer and mix for 15-30min to obtain a primary mixture for later use;
[0049] S2. Pour the mixed material into a Z-type reamer mixer, stir and mix again for 10-20 minutes, then discharge and seal with polyester film to form a mass for storage;
[0050] S3. Heat the mold, then put the mass on the mold, use a 400T press to press, the pressing temperature is controlled at 130-150°C, and the finished product is demoulded and taken out after pressing for 13-17 minutes;
[0051] S4. Use a trimming machine to trim the decorative panels to the required specifications, and conduct quality inspection on the trimmed panels. After passing the inspection, they will be put into storage for future use.
[0052] Example 1
[0053] This embodiment provides a coffee grounds composite decorative board, comprising the following components in parts by weight:
[0054] 500g coffee grounds mixture, 30g nano-silane modified magnesium borate whisker reinforced modified bamboo fiber, 30g phenolic resin, 20g sodium hydroxide, 800g calcium silicate, 220g diatomaceous earth powder, 28g hollow microspheres, 25g wollastonite, 3g water retaining agent, 2g polypropylene fiber, 8g mildew inhibitor, 38g redispersible latex powder, 5g nano zinc powder and 40g water;
[0055] Among them, the coffee grounds mixture is a mixture of coffee grounds, cork particles and polyurethane adhesive, and the mass ratio of the coffee grounds to the cork particles is 80:20; the mass ratio of the polyurethane adhesive to the mixture of coffee grounds and cork particles is 100:30.
[0056] The method for preparing nano-silane modified magnesium borate whisker reinforced modified bamboo fiber comprises the following steps:
[0057] S1. Bamboo fiber pretreatment: 40 g of bamboo fiber was immersed in 1100 mL of a 2% hydrogen peroxide solution by mass, and then sodium hydroxide was gradually added to the mixed solution until the pH value was adjusted to 12-13, followed by immersion at 25 ° C for 4 h to remove impurities, and then placed in a blast drying oven at 80 ° C for 12 h to obtain alkaline hydrogen peroxide pretreated bamboo fiber;
[0058] S2. Modified magnesium borate whisker: 6 g of nano magnesium borate whisker and 12 g of silane coupling agent were dispersed in 100 g of dioxane, ultrasonically dispersed for 30 min, then heated to reflux at 100 ° C for 1.5 h, then centrifuged at 8000 rpm for 15 min to separate the precipitate, and the precipitate was washed 3-5 times with anhydrous ethanol. The washed precipitate was placed in a vacuum drying oven and dried at 135 ° C for 12 h to obtain nano silane coupling agent modified magnesium borate whisker;
[0059] S3. The alkaline hydrogen peroxide pretreated bamboo fiber is placed into the nano-silane coupling agent modified magnesium borate whisker, and then placed in a ball mill to remove the spheres and mixed at 300 rpm for 20 minutes until the mixture is evenly mixed. The obtained bamboo fiber is placed in a vacuum drying oven and dried at 140° C. for 12 hours to obtain the nano-silane modified magnesium borate whisker reinforced modified bamboo fiber.
[0060] This embodiment provides a preparation process of a coffee grounds composite decorative board, comprising the following steps:
[0061] S1. Weigh the raw materials prepared and add them to a high shear mixer and mix for 20 minutes to obtain a primary mixture for later use;
[0062] S2. Pour the mixed material into a Z-type reamer mixer, stir and mix again for 20 minutes before unloading, and seal the package with polyester film to form a mass for storage;
[0063] S3. The mold is heated, and then the mass is molded and pressed using a 400T press. The pressing temperature is controlled at 150°C. After 15 minutes of pressing, the finished product is demoulded and taken out;
[0064] S4. Use a trimming machine to trim the decorative panels to the required specifications, and conduct quality inspection on the trimmed panels. After passing the inspection, they will be put into storage for future use.
[0065] Example 2
[0066] This embodiment provides a coffee grounds composite decorative board, comprising the following components in parts by weight:
[0067] 300g coffee grounds mixture, 20g nano-silane modified magnesium borate whisker reinforced modified bamboo fiber, 30g phenolic resin, 20g sodium hydroxide, 800g calcium silicate, 220g diatomaceous earth powder, 28g hollow microspheres, 25g wollastonite, 3g water retaining agent, 2g polypropylene fiber, 8g mildew inhibitor, 38g redispersible latex powder, 5g nano zinc powder and 40g water;
[0068] Among them, the coffee grounds mixture is a mixture of coffee grounds, cork particles and polyurethane adhesive, and the mass ratio of the coffee grounds to the cork particles is 80:20; the mass ratio of the polyurethane adhesive to the mixture of coffee grounds and cork particles is 100:30.
[0069] The method for preparing nano-silane modified magnesium borate whisker reinforced modified bamboo fiber comprises the following steps:
[0070] S1. Bamboo fiber pretreatment: 40 g of bamboo fiber was immersed in 1100 mL of a 2% hydrogen peroxide solution by mass, and then sodium hydroxide was gradually added to the mixed solution until the pH value was adjusted to 12-13, followed by immersion at 25 ° C for 4 h to remove impurities, and then placed in a blast drying oven at 80 ° C for 12 h to obtain alkaline hydrogen peroxide pretreated bamboo fiber;
[0071] S2. Modified magnesium borate whisker: 6 g of nano magnesium borate whisker and 12 g of silane coupling agent were dispersed in 100 g of dioxane, ultrasonically dispersed for 30 min, then heated to reflux at 100 ° C for 1.5 h, then centrifuged at 8000 rpm for 15 min to separate the precipitate, and the precipitate was washed 3-5 times with anhydrous ethanol. The washed precipitate was placed in a vacuum drying oven and dried at 135 ° C for 12 h to obtain nano silane coupling agent modified magnesium borate whisker;
[0072] S3. The alkaline hydrogen peroxide pretreated bamboo fiber is placed into the nano-silane coupling agent modified magnesium borate whisker, and then placed in a ball mill to remove the spheres and mixed at 300 rpm for 20 minutes until the mixture is evenly mixed. The obtained bamboo fiber is placed in a vacuum drying oven and dried at 140° C. for 12 hours to obtain the nano-silane modified magnesium borate whisker reinforced modified bamboo fiber.
[0073] This embodiment provides a preparation process of a coffee grounds composite decorative board, comprising the following steps:
[0074] S1. Weigh the raw materials prepared and add them to a high shear mixer and mix for 20 minutes to obtain a primary mixture for later use;
[0075] S2. Pour the mixed material into a Z-type reamer mixer, stir and mix again for 20 minutes before unloading, and seal the package with polyester film to form a mass for storage;
[0076] S3. The mold is heated, and then the mass is molded and pressed using a 400T press. The pressing temperature is controlled at 150°C. After 15 minutes of pressing, the finished product is demoulded and taken out;
[0077] S4. Use a trimming machine to trim the decorative panels to the required specifications, and conduct quality inspection on the trimmed panels. After passing the inspection, they will be put into storage for future use.
[0078] Example 3
[0079] This embodiment provides a coffee grounds composite decorative board, comprising the following components in parts by weight:
[0080] 200g coffee grounds mixture, 13g nano-silane modified magnesium borate whisker reinforced modified bamboo fiber, 30g phenolic resin, 20g sodium hydroxide, 800g calcium silicate, 220g diatomaceous earth powder, 28g hollow microspheres, 25g wollastonite, 3g water retaining agent, 2g polypropylene fiber, 8g mildew inhibitor, 38g redispersible latex powder, 5g nano zinc powder and 40g water;
[0081] Among them, the coffee grounds mixture is a mixture of coffee grounds, cork particles and polyurethane adhesive, and the mass ratio of the coffee grounds to the cork particles is 80:20; the mass ratio of the polyurethane adhesive to the mixture of coffee grounds and cork particles is 100:30.
[0082] The method for preparing nano-silane modified magnesium borate whisker reinforced modified bamboo fiber comprises the following steps:
[0083] S1. Bamboo fiber pretreatment: 40 g of bamboo fiber was immersed in 1100 mL of a 2% hydrogen peroxide solution by mass, and then sodium hydroxide was gradually added to the mixed solution until the pH value was adjusted to 12-13, followed by immersion at 25 ° C for 4 h to remove impurities, and then placed in a blast drying oven at 80 ° C for 12 h to obtain alkaline hydrogen peroxide pretreated bamboo fiber;
[0084] S2. Modified magnesium borate whisker: 6 g of nano magnesium borate whisker and 12 g of silane coupling agent were dispersed in 100 g of dioxane, ultrasonically dispersed for 30 min, then heated to reflux at 100 ° C for 1.5 h, then centrifuged at 8000 rpm for 15 min to separate the precipitate, and the precipitate was washed 3-5 times with anhydrous ethanol. The washed precipitate was placed in a vacuum drying oven and dried at 135 ° C for 12 h to obtain nano silane coupling agent modified magnesium borate whisker;
[0085] S3. The alkaline hydrogen peroxide pretreated bamboo fiber is placed into the nano-silane coupling agent modified magnesium borate whisker, and then placed in a ball mill to remove the spheres and mixed at 300 rpm for 20 minutes until the mixture is evenly mixed. The obtained bamboo fiber is placed in a vacuum drying oven and dried at 140° C. for 12 hours to obtain the nano-silane modified magnesium borate whisker reinforced modified bamboo fiber.
[0086] This embodiment provides a preparation process of a coffee grounds composite decorative board, comprising the following steps:
[0087] S1. Weigh the raw materials prepared and add them to a high shear mixer and mix for 20 minutes to obtain a primary mixture for later use;
[0088] S2. Pour the mixed material into a Z-type reamer mixer, stir and mix again for 20 minutes before unloading, and seal the package with polyester film to form a mass for storage;
[0089] S3. The mold is heated, and then the mass is molded and pressed using a 400T press. The pressing temperature is controlled at 150°C. After 15 minutes of pressing, the finished product is demoulded and taken out;
[0090] S4. Use a trimming machine to trim the decorative panels to the required specifications, and conduct quality inspection on the trimmed panels. After passing the inspection, they will be put into storage for future use.
[0091] Comparative Example 1: This example is used as a comparative example of Example 1, except that the nano-silane-modified magnesium borate whisker-reinforced modified bamboo fiber is replaced with wood fiber, and the other steps and parameters are the same as those of Example 1.
[0092] Comparative Example 2: This example is a comparative example of Example 1, except that the coffee grounds mixture in the formula is removed, and the other steps and parameters are the same as those in Example 1.
[0093] Test: The decorative panels prepared in Examples 1-3 and Comparative Example 1 were subjected to performance tests, the oxygen index was tested according to GB / T2406-1993, the heat deformation temperature was tested according to GB / T1634.2-2004, the tensile strength was tested according to GB / T1040-2006; the notched impact strength was tested according to GB / T1843-1996; the results are shown in Table 1.
[0094] Table 1 Comparison of decorative board material performance test results
[0095]
[0096] in conclusion:
[0097] 1. The heat deformation temperatures of Examples 1-3 are significantly higher than those of Comparative Examples 1 and 2, indicating that under a higher temperature environment, the decorative board using a mixture of nano-silane-modified magnesium borate whiskers reinforced with modified bamboo fiber and coffee grounds has better dimensional stability and is less likely to deform. However, since Comparative Example 1 uses wood fiber instead of reinforced modified bamboo fiber, its heat deformation temperature is significantly reduced, indicating that the dimensional stability of wood fiber at high temperatures is poor.
[0098] 2. The tensile strength of Examples 1-3 is significantly higher than that of Comparative Examples 1 and 2, indicating that the decorative board using nano-silane modified magnesium borate whiskers to reinforce modified bamboo fiber and coffee grounds mixture has higher mechanical strength and can withstand greater tensile loads without damage. Since Comparative Example 1 uses wood fiber and Comparative Example 2 does not use a coffee grounds mixture, its tensile strength is significantly lower than that of Examples 1-3, indicating that wood fiber is not as good as reinforced modified bamboo fiber in enhancing the strength of the board, and the cellulose and hemicellulose components contained in the coffee grounds mixture enhance the mechanical strength and toughness of the board, and play a positive role in enhancing the tensile strength of the decorative board.
[0099] 3. The notched impact strength of Examples 1-3 is higher than that of Comparative Example 1, indicating that the decorative board using the coffee grounds mixture and nano-silane modified magnesium borate whisker reinforced modified bamboo fiber is not easy to crack or break when impacted, and has better impact resistance. However, since Comparative Example 1 uses wood fiber, its notched impact strength is lower, indicating that wood fiber is not as good as reinforced modified bamboo fiber in improving the impact resistance of the board.
[0100] 4. The oxygen index of Examples 1-3 is significantly higher than that of Comparative Examples 1 and 2, indicating that the decorative board using nano-silane modified magnesium borate whisker to reinforce modified bamboo fiber has better flame retardant properties and can provide higher safety in fires, and the coffee grounds mixture has the characteristics of moisture absorption and air permeability, which also plays a positive role in the flame retardant properties of the decorative board. Comparative Example 1 uses wood fiber, so its oxygen index is lower, indicating that wood fiber is not as good as reinforced modified bamboo fiber in improving the flame retardant properties of the board.
[0101] In summary, the decorative panels prepared by Examples 1-3 are superior to those of Comparative Examples 1 and 2 in terms of heat deformation temperature, tensile strength, notched impact strength and oxygen index. This shows that the decorative panels using nano-silane modified magnesium borate whiskers to reinforce modified bamboo fibers have better comprehensive performance and are suitable for applications requiring higher heat resistance, mechanical strength, impact resistance and flame retardancy. However, due to the use of wood fiber, the performance of Comparative Example 1 is relatively weak, indicating that the reinforced modified bamboo fiber plays an important role in improving the performance of the decorative panels. In addition, the addition of the coffee grounds mixture not only realizes the resource utilization of waste, but also further enhances the performance of the board through its own characteristics. The overall synergistic effect of the formula makes the board perform well in many aspects and has broad application prospects.
[0102] Although the present invention has been described in detail above by general description and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements can be made to the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all belong to the scope of protection claimed by the present invention.
Claims
1. A coffee grounds composite decorative board, characterized in that: It comprises the following components in parts by weight: 200-500 parts of coffee grounds mixture, 13-30 parts of nano-silane-modified magnesium borate whisker reinforced modified bamboo fiber, 15-35 parts of phenolic resin, 10-20 parts of sodium hydroxide, 600-900 parts of calcium silicate, 120-240 parts of diatomaceous earth powder, 12-36 parts of hollow microbeads, 15-25 parts of wollastonite, 1-3 parts of water-retaining agent, 0.5-2 parts of polypropylene fiber, 6-12 parts of mildew inhibitor, 32-46 parts of redispersible latex powder, 1-5 parts of nano-zinc powder and 20-40 parts of water; The coffee grounds mixture is formed by mixing coffee grounds, cork particles and polyurethane adhesive, wherein the mass ratio of the coffee grounds to the cork particles is (80-90):(10-20); the mass ratio of the polyurethane adhesive to the mixture of coffee grounds and cork particles is (80-120):(20-40).
2. The coffee grounds composite decorative board according to claim 1, characterized in that: The preparation method of the nano-silane modified magnesium borate whisker reinforced modified bamboo fiber comprises the following steps: S1 bamboo fiber pretreatment: The bamboo fiber was immersed in a hydrogen peroxide solution, impregnated to remove impurities, and then placed in a blast drying oven for drying to obtain alkaline hydrogen peroxide pretreated bamboo fiber; S2. Modified magnesium borate whiskers: Nano-magnesium borate whiskers and a silane coupling agent were dispersed in dioxane, ultrasonically dispersed, and then heated under reflux at 100-110°C for 0.5-1.5h. The precipitate was then separated by centrifugation, washed with anhydrous ethanol, and finally dried to obtain nano-silane coupling agent-modified magnesium borate whiskers; S3. Bamboo fiber pretreated with alkaline hydrogen peroxide is placed in nano-silane coupling agent-modified magnesium borate whiskers, and then placed in a ball mill to mix evenly. The resulting bamboo fiber is placed in a vacuum drying oven and dried at 135-145°C for 12-15 hours to obtain nano-silane-modified magnesium borate whisker-reinforced modified bamboo fiber.
3. The coffee grounds composite decorative board according to claim 2, characterized in that: In the S1, the bamboo fiber is 25-40 parts by weight, the hydrogen peroxide solution is 800-1200 mL, and the mass fraction of the hydrogen peroxide solution is 1-3%.
4. The coffee grounds composite decorative board according to claim 3, characterized in that: In S1, the bamboo fibers are immersed in a hydrogen peroxide solution, and then sodium hydroxide is gradually added to the mixed solution until the pH value is adjusted to 12-13.
5. The coffee grounds composite decorative board according to claim 4, characterized in that: In S1, the immersion temperature is 25-35°C and the immersion time is 2-4 hours; The drying temperature in the blast drying oven is 70-110° C., and the drying time is 8-12 hours.
6. The coffee grounds composite decorative board according to claim 2, characterized in that: The silane coupling agent in S2 is one or more of γ-glycidoxypropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-chloropropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, and 3-isocyanatepropyltriethoxysilane.
7. The coffee grounds composite decorative board according to claim 6, characterized in that: The S2 contains 4-7 parts by weight of nano magnesium borate whiskers, 9-16 parts by weight of silane coupling agent, and 80-100 parts by weight of dioxane.
8. The coffee grounds composite decorative board according to claim 7, characterized in that: In the S2, the ultrasonic dispersion time is 10-30 minutes; the heating reflux temperature is 90-110° C., the time is 0.5-2.5 hours; the centrifugal speed is 5000-10000 rpm, and the centrifugal time is 5-15 minutes.
9. The coffee grounds composite decorative board according to claim 8, characterized in that: In the step S2, the separated precipitate is washed 3-5 times with anhydrous ethanol, and the washed precipitate is placed in a vacuum drying oven and dried at 135-145° C. for 12-15 hours.
10. A process for preparing a coffee grounds composite decorative board, for preparing the coffee grounds composite decorative board according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1 weighed the raw materials prepared and added to a high shear mixer and mixed for 15-30min to obtain a primary mixture for later use; S2. The mixed material is poured into a Z-type reamer mixer, stirred and mixed again for 10-20min before unloading, and sealed with polyester film to form a mass for storage; S3. The mold is heated, and then the mass is molded and pressed using a 400T press. The pressing temperature is controlled at 130-150°C, and the finished product is removed from the mold after 13-17min pressing. S4. Use a trimming machine to trim the decorative panels to the required specifications, and conduct quality inspection on the trimmed panels. Once qualified, they will be put into storage for future use.
Citation Information
Patent Citations
Method for surface modification of magnesium borate crystal whisker by using borate coupling agent
CN102321395A
Calcium silicate board and preparation method thereof
CN107473681A
Coffee cork and preparation method and application thereof
CN111070367A
Biodegradable composition
WO2020047816A1