Gel-casting silica gel mold and preparation method thereof

By adjusting the thickness of the inner and outer layers of the silicone mold and the ratio of raw materials, using modified nanoparticles and calcium stearate, the strength and toughness of the mold are improved, and the problems of short service life and low accuracy of the silicone mold are solved, and large size is achieved , The production demand for high-precision injection molding materials reduces production costs.

CN119081409AInactive Publication Date: 2024-12-06SHANDONG UNIV OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411231148.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing silicone molds have short service life and low dimensional accuracy, making it difficult to meet the production needs of large-size and high-precision injection molding materials.

Method used

By adjusting the thickness relationship between the inner and outer layers of the mold and the ratio of raw materials, and using modified nanoparticles and calcium stearate, the strength and toughness of the mold are improved, ensuring high accuracy and long life.

Benefits of technology

It significantly improves the service life and dimensional accuracy of the mold, reduces production costs, reduces deformation and crack problems, and increases the number of use to 2.5 to 3 times that of ordinary silicone molds.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081409A_ABST
    Figure CN119081409A_ABST
Patent Text Reader

Abstract

The invention provides a gel casting silica gel mold and a preparation method thereof, and relates to the technical field of gel casting. The gel casting silica gel mold sequentially comprises an inner layer and an outer layer from inside to outside, the thickness of the inner layer is 20%-50% of the total thickness of the mold, and the thickness of the outer layer is 50%-80% of the total thickness of the mold; the outer layer is prepared from vinyl-terminated silicone oil, an antioxidant, a curing agent and a silica gel matrix; the inner layer is composed of vinyl-terminated silicone oil, modified nanoparticles, calcium stearate, an antioxidant, a curing agent and a silica gel matrix. The invention also provides a preparation method of the nanoparticle. By adjusting the thickness relation of the inner layer and the outer layer of the mold and the ratio of the raw materials, the mold has the advantages of high strength and high toughness, the service life of the mold is remarkably prolonged, and the production cost of the gel casting material which is complex in structure and has the characteristics of large size and high precision is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of gel injection molding, and in particular to a gel injection molding silicone mold and a preparation method thereof. Background Art

[0002] Gel injection molding is a technology based on the in-situ polymerization of organic monomer binders to form a polymer network, which condenses powder particles together. Gel injection molding has been successfully used to produce coarse-grained ceramics, advanced refractory materials, ceramic composites, structural ceramics, functional and bioceramics, porous materials and powder metallurgy. Gel injection molding has no special requirements for powders, and can produce large-sized, complex-shaped and thick-walled parts. The mold can be made of a variety of materials, with a short molding cycle, high strength of wet and dry billets, and can be machined. The billet has a low organic content, and the performance of the billet and sintered body is uniform. The process is easy to control, the process and operation are relatively simple, the equipment is simple, and the cost is low. Compared with other molding technologies, the gel injection molding process has many advantages that traditional molding processes cannot achieve.

[0003] An important step in gel injection molding is molding and demoulding. Silicone molds are one of the molds that can be selected in the gel injection molding process. Silicone molds have good elasticity and can be easily demoulded. They are suitable for products with complex shapes and rich details. They have low production costs and short production time, and can be put into production quickly. However, due to the high viscosity and weight of the gel injection molding slurry itself, the service life of silicone molds is short. Due to the characteristics of the material, the dimensional accuracy of silicone molds is low, which is not suitable for the preparation of products with high precision requirements.

[0004] Therefore, it is necessary to develop an injection molding mold with high strength, high toughness, long service life, and can meet the requirements of large-size and high-precision preparation. Summary of the invention

[0005] In view of this, the present invention provides a gel injection molding silicone mold and a preparation method thereof. The present invention adjusts the thickness relationship between the inner and outer layers of the mold and the ratio of the raw materials so that the mold has the advantages of high strength and high toughness, significantly improves the service life of the mold, and reduces the production cost of gel injection molding materials with complex structures, large sizes, and high precision characteristics.

[0006] The gel injection molding silicone mold of the present invention comprises an inner layer and an outer layer from inside to outside, the thickness of the inner layer is 20% to 50% of the total thickness of the mold, and the thickness of the outer layer is 50% to 80% of the total thickness of the mold.

[0007] Furthermore, the outer layer is composed of the following raw materials in percentage by mass: 4-10% of vinyl-terminated silicone oil, 1-2% of antioxidant, 1-3% of curing agent, and the remainder is a silicone matrix.

[0008] Furthermore, the inner layer is composed of the following raw materials in percentage by mass: 4-10% of vinyl-terminated silicone oil, 1-10% of modified nanoparticles, 1-3% of calcium stearate, 1-2% of antioxidant, 1-3% of curing agent, and the remainder is a silica gel matrix.

[0009] The preparation method of the modified nanoparticles is as follows:

[0010] The nano-silicon dioxide and nano-aluminum oxide are mixed uniformly in proportion and then dried to obtain mixed nano-particles, and then a silane coupling agent and xylene are added to the mixed nano-particles for modification, and after the modification is completed, the mixture is filtered, washed, and dried to obtain modified nano-particles;

[0011] Furthermore, the mass ratio of the nano-silicon dioxide to the nano-aluminum oxide is (3-5):(0.5-1.5). Preferably, the mass ratio of the nano-silicon dioxide to the nano-aluminum oxide is 4:1.

[0012] Furthermore, the drying temperature of the mixed nanoparticles is 180° C. to 200° C., and the drying time is 10 to 20 hours. Preferably, the drying temperature of the mixed nanoparticles is 185° C., and the drying time is 15 hours.

[0013] Furthermore, the amount of the silane coupling agent added is 0.5 wt.% to 1.5 wt.% of the mixed nanoparticles. Preferably, the amount of the silane coupling agent added is 1.0 wt.% of the mixed nanoparticles.

[0014] Further, the mass ratio of the mixed nanoparticles to the xylene is 1:(0.5-5). Preferably, the mass ratio of the mixed nanoparticles to the xylene is 1:(2-3). More preferably, the mass ratio of the mixed nanoparticles to the xylene is 1:2.5.

[0015] Furthermore, the modification temperature is 100°C to 120°C, and the modification time is 3 to 7 hours. Preferably, the modification temperature is 110°C, and the modification time is 5 hours.

[0016] Furthermore, the silane coupling agent is silane coupling agent KH-560 and silane coupling agent KH-570, and the mass ratio of the silane coupling agent KH-560 to the silane coupling agent KH-570 is (1-2):(4-5). Preferably, the mass ratio of the silane coupling agent KH-560 to the silane coupling agent KH-570 is 1.5:4.5.

[0017] Furthermore, the antioxidant is antioxidant 1010.

[0018] The present invention also provides a method for preparing the gel injection molding silicone mold, comprising the following steps:

[0019] S1. Weighing raw materials according to proportion to prepare modified nanoparticles;

[0020] S2, weighing raw materials according to proportion, and preparing outer layer raw materials and inner layer raw materials respectively;

[0021] S3, adding the outer layer raw material into the pressing mold, extruding and molding, pouring the inner layer raw material into the mold after the outer layer material is about to solidify, and demoulding after solidification to obtain an injection molding silicone mold.

[0022] Compared with the prior art, the beneficial technical effects of the present invention are:

[0023] The present invention adjusts the thickness of the inner and outer layers of the mold and the ratio of raw materials so that the mold has both high strength and toughness, can better meet the preparation requirements of complex-shaped injection molding materials, improve the dimensional accuracy of the mold, and significantly reduce the production cost of complex, large-sized, and high-precision injection molding materials.

[0024] The present invention effectively prevents deformation caused by poor strength of silicone during the preparation of large-size and high-precision materials by optimizing the material ratio.

[0025] The invention significantly increases the service life of the mold, reduces the occurrence of problems such as cracks or surface ruptures, and the number of uses is 2.5 to 3 times that of ordinary silicone molds. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The present invention will be further described below in conjunction with the accompanying drawings.

[0027] Figure 1 This is a process flow chart for preparing the injection molding silicone mold of the present invention. DETAILED DESCRIPTION

[0028] The invention provides a gel injection molding silicone mold, which comprises an inner layer and an outer layer from inside to outside, wherein the thickness of the inner layer is 20% to 50% of the total thickness of the mold, and the thickness of the outer layer is 50% to 80% of the total thickness of the mold.

[0029] The present invention strictly limits the thickness distribution of the outer layer and the inner layer in the whole. First, the preparation process of the inner layer raw material is relatively complicated and costly. However, the setting of the inner layer can significantly improve the strength and toughness of the mold, and is the main means to ensure the accuracy of the mold and increase its service life. Therefore, taking into account both the cost and the effect, the present invention limits the thickness of the inner layer to 20% to 50% of the total thickness of the mold, and the thickness of the outer layer to 50% to 80% of the total thickness of the mold.

[0030] In one embodiment, the outer layer is composed of the following raw materials in percentage by mass: 4-10% vinyl-terminated silicone oil, 1-2% antioxidant, 1-3% curing agent, and the remainder is a silicone matrix.

[0031] In one embodiment, the inner layer is composed of the following raw materials in percentage by mass: 4-10% vinyl-terminated silicone oil, 1-10% modified nanoparticles, 1-3% calcium stearate, 1-2% antioxidant, 1-3% curing agent, and the remainder is a silica gel matrix.

[0032] The vinyl structure of vinyl-terminated silicone oil makes it highly reactive, which can significantly improve the strength and toughness of silicone. In addition, vinyl-terminated silicone oil can also improve the fluidity and formability of silicone, making it easier to process and shape during mold manufacturing.

[0033] In addition, limiting the content of the vinyl-terminated silicone oil to 4-10% can achieve a balance between the comprehensive performance of the mold and the processing performance, and can maintain good processing properties and cost-effectiveness while ensuring performance.

[0034] In one embodiment, the preparation method of the nano-modified silicon dioxide is as follows:

[0035] Nano-silicon dioxide and nano-aluminum oxide are mixed uniformly in proportion and then dried to obtain mixed nano-particles. Then, a silane coupling agent and xylene are added to the mixed nano-particles for modification. After the modification, the mixed nano-particles are filtered, washed with acetone, and dried to obtain modified nano-particles.

[0036] In one embodiment, the mass ratio of the nano-silicon dioxide to the nano-aluminum oxide is (3-5):(0.5-1.5).

[0037] In one embodiment, the mass ratio of the nano-silicon dioxide to the nano-aluminum oxide is 4:1.

[0038] The present invention focuses on the use of modified nanoparticles. First, the present invention selects nano-silicon dioxide and nano-aluminum oxide to prepare the mold. Among them, nano-silicon dioxide provides excellent strength because it has a high specific surface area, can form more interface bonding forces in the material, and reduce stress concentration by filling tiny pores and defects, thereby enhancing the overall strength of the material. At the same time, the interface interaction between nano-silicon dioxide and the matrix material is significant, which further improves the strength of the material. On the other hand, nano-aluminum oxide enhances toughness because it can cause cracks to deflect and bifurcate when the material breaks, consumes fracture energy, and has a higher elastic modulus, which can provide better stress dispersion effect. In addition, nano-aluminum oxide can also form fine whiskers or particles in the material, improve the microstructure of the material, and further improve its toughness. These characteristics enable nano-silicon dioxide and nano-aluminum oxide to provide excellent strength and toughness respectively in composite materials to meet the needs of high-performance materials.

[0039] The present invention also defines the mass ratio of nano silicon dioxide and nano aluminum oxide, the main purpose of which is to achieve the best balance between strength and toughness. In addition, this ratio helps to evenly disperse the nanoparticles in the matrix material, avoid agglomeration, and thus improve the overall performance of the material. Experiments show that the ratio range of (3 to 5): (0.5 to 1.5) can maximize the advantages of the two nanomaterials and improve the mechanical properties and thermal stability of the material. Within this ratio range, the performance of the material can be guaranteed and the cost can be controlled, making it more economical in practical applications. The selection of this ratio is based on a large number of experiments and performance tests to ensure that the material achieves the best balance in strength, toughness, dispersibility and thermal stability.

[0040] In one embodiment, the drying temperature of the mixed nanoparticles is 180° C. to 200° C., and the drying time is 10 to 20 hours.

[0041] In one embodiment, the drying temperature of the hybrid nanoparticles is 185° C., and the drying time is 15 h.

[0042] In one embodiment, the added amount of the silane coupling agent is 0.5 wt. % to 1.5 wt. % of the hybrid nanoparticles.

[0043] In one embodiment, the added amount of the silane coupling agent is 1.0 wt. % of the hybrid nanoparticles.

[0044] Furthermore, the mass ratio of the mixed nanoparticles to the xylene is 1:(0.5-5).

[0045] In one embodiment, the mass ratio of the mixed nanoparticles to the xylene is 1:(2-3).

[0046] In one embodiment, the mass ratio of the mixed nanoparticles to the xylene is 1:2.5.

[0047] In one embodiment, the modification temperature is 100° C. to 120° C., and the modification time is 3 to 7 hours. Preferably, the modification temperature is 110° C., and the modification time is 5 hours.

[0048] In one embodiment, the silane coupling agent is silane coupling agent KH-560 and silane coupling agent KH-570, and the mass ratio of the silane coupling agent KH-560 to the silane coupling agent KH-570 is (1-2):(4-5).

[0049] In one embodiment, the mass ratio of the silane coupling agent KH-560 to the silane coupling agent KH-570 is 1.5:4.5.

[0050] The present invention strictly limits the types of silane coupling agents in the process of nanoparticle modification, wherein: silane coupling agent KH-560 is γ-(2,3-epoxypropoxy)propyltrimethoxysilane, and silane coupling agent KH-570 is γ-methacryloxypropyltrimethoxysilane. In the present invention, the epoxy group in γ-(2,3-epoxypropoxy)propyltrimethoxysilane can significantly improve the strength of silica gel, and enhance its mechanical strength, wear resistance and durability. On the other hand, the methacryloxy group in γ-methacryloxypropyltrimethoxysilane can improve the toughness of silica gel. Moreover, by improving the dispersibility and compatibility of silica gel, KH-570 can effectively disperse nanoparticles and enhance the toughness of the material.

[0051] In addition, the present invention also strictly limits the mass ratio of the two silane coupling agents, thereby regulating the ratio of the modified nanoparticles, ensuring the uniform distribution of the epoxy group and the methacryloyloxy group in the material, optimizing the dispersion of the nanoparticles in the silica gel matrix, and maximizing the advantages of the two coupling agents to improve the mechanical properties, weather resistance and chemical resistance of the material. At the same time, the cost-effectiveness of the material is considered to ensure that the performance is improved while maintaining a reasonable cost.

[0052] Finally, the ratio of the above silane coupling agent can ensure good bonding between the outer layer and the inner layer and will not separate during use.

[0053] In one embodiment, the antioxidant is antioxidant 1010 .

[0054] A certain amount of calcium stearate is also added to the inner layer raw material of the present invention, which helps the subsequent demoulding, reduces the demoulding difficulty, can protect the mold, and improve the service life of the mold.

[0055] The present invention also provides a method for preparing the gel injection molding silicone mold, comprising the following steps:

[0056] S1. Weighing raw materials according to proportion to prepare modified nanoparticles;

[0057] S2, weighing raw materials according to proportion, and preparing outer layer raw materials and inner layer raw materials respectively;

[0058] S3, adding the outer layer raw material into the pressing mold, extruding and molding, pouring the inner layer raw material into the mold after the outer layer material is about to solidify, and demoulding after solidification to obtain an injection molding silicone mold.

[0059] The technical solution provided by the present invention is further described below in conjunction with embodiments.

[0060] Embodiment 1 A gel injection molding silicone mold comprises an inner layer and an outer layer from the inside to the outside, wherein the thickness of the inner layer is 35% of the total thickness of the mold, and the thickness of the outer layer is 65% of the total thickness of the mold.

[0061] The outer layer is composed of the following raw materials in percentage by mass: 5% of vinyl-terminated silicone oil, 10102% of antioxidant, 3% of silicone curing agent, and the remainder is silicone matrix.

[0062] The inner layer is composed of the following raw materials in percentage by mass: 5% of vinyl-terminated silicone oil, 5% of modified nanoparticles, 3% of calcium stearate, 10102% of antioxidant, 3% of silicone curing agent, and the remainder is silicone matrix.

[0063] The nanoparticles are composed of nano silicon dioxide and nano aluminum oxide in a mass ratio of 4:1.

[0064] The preparation method of the nano-modified silicon dioxide is as follows:

[0065] The nano-silicon dioxide and nano-alumina are uniformly mixed in a mass ratio of 3:1.5, and then dried at 185° C. for 15 hours to obtain mixed nano-particles, and then 1.0 wt.% of a silane coupling agent and xylene 2.5 times the weight of the mixed nano-particles are added to the mixed nano-particles, and modified at 110° C. for 5 hours. After the modification is completed, the mixture is filtered, washed with acetone to remove unreacted nano-particles, and dried to obtain modified nano-particles;

[0066] The silane coupling agent is composed of silane coupling agent KH-560 and silane coupling agent KH-570 in a mass ratio of 1.5:4.5.

[0067] The preparation method of the injection molding silicone mold comprises the following steps:

[0068] S1. Weighing raw materials according to proportion to prepare modified nanoparticles;

[0069] S2, weighing raw materials according to proportion, and preparing outer layer raw materials and inner layer raw materials respectively;

[0070] S3, adding the outer layer raw material into the pressing mold, extruding and molding, pouring the inner layer raw material into the mold after the outer layer material is about to solidify (80% of the solidification time, the solidification time can be measured by experiment), and demoulding after solidification to obtain an injection molding silicone mold.

[0071] Embodiment 2 is an injection molding silicone mold, which comprises an inner layer and an outer layer from the inside to the outside, wherein the thickness of the inner layer is 50% of the total thickness of the mold, and the thickness of the outer layer is 50% of the total thickness of the mold.

[0072] The outer layer is composed of the following raw materials in percentage by mass: 4% of vinyl-terminated silicone oil, 10101% of antioxidant, 1% of silicone curing agent, and the remainder is silicone matrix.

[0073] The inner layer is composed of the following raw materials in percentage by mass: 4% of vinyl-terminated silicone oil, 1% of modified nanoparticles, 1% of calcium stearate, 10101% of antioxidant, 1% of silicone curing agent, and the remainder is silicone matrix.

[0074] The nanoparticles are composed of nano silicon dioxide and nano aluminum oxide in a mass ratio of 4:1.

[0075] The preparation method of the nano-modified silicon dioxide is as follows:

[0076] The nano-silicon dioxide and nano-alumina are uniformly mixed in a mass ratio of 3:1.5, and then dried at 185° C. for 15 hours to obtain mixed nano-particles, and then 1.0 wt.% of a silane coupling agent and xylene 2.5 times the weight of the mixed nano-particles are added to the mixed nano-particles, and modified at 110° C. for 5 hours. After the modification is completed, the mixture is filtered, washed with acetone to remove unreacted nano-particles, and dried to obtain modified nano-particles;

[0077] The silane coupling agent is composed of silane coupling agent KH-560 and silane coupling agent KH-570 in a mass ratio of 1.5:4.5.

[0078] The preparation method of the injection molding silicone mold comprises the following steps:

[0079] S1. Weighing raw materials according to proportion to prepare modified nanoparticles;

[0080] S2, weighing raw materials according to proportion, and preparing outer layer raw materials and inner layer raw materials respectively;

[0081] S3, adding the outer layer raw material into the pressing mold, extruding and molding, pouring the inner layer raw material into the mold after the outer layer material is about to solidify (80% of the solidification time, the solidification time can be measured by experiment), and demoulding after solidification to obtain an injection molding silicone mold.

[0082] Embodiment 3 is an injection molding silicone mold, which comprises an inner layer and an outer layer from the inside to the outside, wherein the thickness of the inner layer is 20% of the total thickness of the mold, and the thickness of the outer layer is 80% of the total thickness of the mold.

[0083] The outer layer is composed of the following raw materials in percentage by mass: 10% of vinyl-terminated silicone oil, 10102% of antioxidant, 3% of silicone curing agent, and the remainder is silicone matrix.

[0084] The inner layer is composed of the following raw materials in percentage by mass: 10% of vinyl-terminated silicone oil, 10% of modified nanoparticles, 3% of calcium stearate, 10103% of antioxidant, 3% of silicone curing agent, and the remainder is silicone matrix.

[0085] The nanoparticles are composed of nano silicon dioxide and nano aluminum oxide in a mass ratio of 4:1.

[0086] The preparation method of the nano-modified silicon dioxide is as follows:

[0087] The nano-silicon dioxide and nano-alumina are uniformly mixed in a mass ratio of 3:1.5, and then dried at 185° C. for 15 hours to obtain mixed nano-particles, and then 1.0 wt.% of a silane coupling agent and xylene 2.5 times the weight of the mixed nano-particles are added to the mixed nano-particles, and modified at 110° C. for 5 hours. After the modification is completed, the mixture is filtered, washed with acetone to remove unreacted nano-particles, and dried to obtain modified nano-particles;

[0088] The silane coupling agent is composed of silane coupling agent KH-560 and silane coupling agent KH-570 in a mass ratio of 1.5:4.5.

[0089] The preparation method of the injection molding silicone mold comprises the following steps:

[0090] S1. Weighing raw materials according to proportion to prepare modified nanoparticles;

[0091] S2, weighing raw materials according to proportion, and preparing outer layer raw materials and inner layer raw materials respectively;

[0092] S3, adding the outer layer raw material into the pressing mold, extruding and molding, pouring the inner layer raw material into the mold after the outer layer material is about to solidify (80% of the solidification time, the solidification time can be measured by experiment), and demoulding after solidification to obtain an injection molding silicone mold.

[0093] Comparative Example 1

[0094] Same as Example 1, except that calcium stearate is not included in the inner layer raw materials.

[0095] Comparative Example 2

[0096] Same as Example 1, except that the modified nanoparticles are modified nano-silicon dioxide.

[0097] Comparative Example 3

[0098] Same as Example 1, except that the modified nanoparticles are modified nano-alumina.

[0099] Comparative Example 4

[0100] The same as Example 1, except that the nanoparticles are composed of nano-silicon dioxide and nano-aluminum oxide in a mass ratio of 6:1.5.

[0101] Comparative Example 5

[0102] The same as Example 1, except that the nanoparticles are composed of nano silicon dioxide and nano aluminum oxide in a mass ratio of 4:3.

[0103] Comparative Example 6

[0104] Same as Example 1, except that the silane coupling agent is silane coupling agent KH-560.

[0105] Comparative Example 7

[0106] Same as Example 1, except that the silane coupling agent is silane coupling agent KH-570.

[0107] Comparative Example 8

[0108] The same as Example 1, except that: the silane coupling agent is composed of silane coupling agent KH-560 and silane coupling agent KH-570 in a mass ratio of 1:6.

[0109] Comparative Example 9

[0110] The same as Example 1, except that: the silane coupling agent is composed of silane coupling agent KH-560 and silane coupling agent KH-570 in a mass ratio of 3:4.

[0111] Test Example 1

[0112] The creative graphics and surface textures of the graphics, animal skin and hair, and concave and convex surfaces of the artistic creation were made into models, and then made into large-scale (1m×1m×0.8m) injection molding silicone molds with a thickness of 10cm. A control group was set up: 5% of vinyl-terminated silicone oil, 10102% of antioxidant, 3% of silicone curing agent, and the rest was silicone matrix.

[0113] Grouting material: uniformly mix acrylamide and N,N-methylene acrylamide in a weight percentage ratio of 20:3, and then take the mixture and dissolve it in distilled water at a ratio of 1g / 10mL to prepare a premixed solution; take the premixed solution, add 10% (v / v) ammonia water, and then add 10% (v / v) 30% sodium polyacrylate aqueous solution, mix evenly, add 5g / mL stone powder with a particle size of 200μm, and then ball mill to prepare stone powder injection molding slurry; take the stone powder injection molding slurry, 100mL, add 1% (v / v) 5% ammonium persulfate initiator, and then add 1% (v / v) N,N,N,N-tetraethylenediamine catalyst, quickly stir evenly, and immediately inject into the mold, wait for it to be completely cured at 100°C, demold and dry.

[0114] The usage times of the molds of Examples 1-3, Comparative Examples 1-9 and the Control Group were tested, and the results are shown in Table 1.

[0115] SPSS Statistics 26 was used for statistical analysis. The results were expressed as x±s. Two-tailed t-test was used to analyze relevant experimental data. Each experiment was repeated at least three times, and P<0.05 was considered statistically significant.

[0116] Use times Dimensional accuracy Control group 31.67±1.26 Severe deformation, severe loss of details Example 1 <![CDATA[82.67±1.12 ** ]]> Good, complete details Example 2 <![CDATA[80.33±0.61 ** ]]> Good, complete details Example 3 <![CDATA[82.67±0.89 ** ]]> Good, complete details Comparative Example 1 <![CDATA[71.00±1.45 △△ ]]> Good, complete details Comparative Example 2 <![CDATA[53.67±1.94 △△ ]]> Good, complete details Comparative Example 3 <![CDATA[80.33±1.30 △ ]]> Severe distortion, loss of detail Comparative Example 4 <![CDATA[61.33±0.58 △△ ]]> Good, complete details Comparative Example 5 <![CDATA[84.67±2.13 △ ]]> Slight distortion, loss of detail Comparative Example 6 <![CDATA[56.67±1.27 △△ ]]> Good, complete details Comparative Example 7 <![CDATA[80.67±2.02 △ ]]> Slight distortion, blurred details Comparative Example 8 81.67±2.29 Slight distortion, blurred details Comparative Example 9 <![CDATA[64.67±1.76 △△ ]]> Good, complete details

[0117] * Compared with the control group, P < 0.05. ** Compared with the control group, P < 0.01. △ Compared with Example 1, P < 0.05, △△ Compared with Example 1, P<0.01.

[0118] In addition, during the test, there was a slight separation between the inner and outer layers of Comparative Examples 6 and 7, but it did not affect the use of the mold.

[0119] Embodiment 4 is an injection molding silicone mold, which comprises an inner layer and an outer layer from the inside to the outside, wherein the thickness of the inner layer is 35% of the total thickness of the mold, and the thickness of the outer layer is 65% of the total thickness of the mold.

[0120] The outer layer is composed of the following raw materials in percentage by mass: 5% of vinyl-terminated silicone oil, 10102% of antioxidant, 3% of silicone curing agent, and the remainder is silicone matrix.

[0121] The inner layer is composed of the following raw materials in percentage by mass: 5% of vinyl-terminated silicone oil, 5% of modified nanoparticles, 3% of calcium stearate, 10102% of antioxidant, 3% of silicone curing agent, and the remainder is silicone matrix.

[0122] The nanoparticles are composed of nano silicon dioxide and nano aluminum oxide in a mass ratio of 4:1.

[0123] The preparation method of the nano-modified silicon dioxide is as follows:

[0124] The nano-silicon dioxide and nano-alumina are uniformly mixed in a mass ratio of 5:0.5, and then dried at 185° C. for 15 hours to obtain mixed nano-particles, and then 1.0 wt.% of a silane coupling agent and xylene 2.5 times the weight of the mixed nano-particles are added to the mixed nano-particles, and modified at 110° C. for 5 hours. After the modification is completed, the mixture is filtered, washed with acetone to remove unreacted nano-particles, and dried to obtain modified nano-particles;

[0125] The silane coupling agent is composed of silane coupling agent KH-560 and silane coupling agent KH-570 in a mass ratio of 1.5:4.5.

[0126] The preparation method of the injection molding silicone mold comprises the following steps:

[0127] S1. Weighing raw materials according to proportion to prepare modified nanoparticles;

[0128] S2, weighing raw materials according to proportion, and preparing outer layer raw materials and inner layer raw materials respectively;

[0129] S3, adding the outer layer raw material into the pressing mold, extruding and molding, pouring the inner layer raw material into the mold after the outer layer material is about to solidify (80% of the solidification time, the solidification time can be measured by experiment), and demoulding after solidification to obtain an injection molding silicone mold.

[0130] Embodiment 5 is an injection molding silicone mold, which comprises an inner layer and an outer layer from the inside to the outside, wherein the thickness of the inner layer is 35% of the total thickness of the mold, and the thickness of the outer layer is 65% of the total thickness of the mold.

[0131] The outer layer is composed of the following raw materials in percentage by mass: 5% of vinyl-terminated silicone oil, 10102% of antioxidant, 3% of silicone curing agent, and the remainder is silicone matrix.

[0132] The inner layer is composed of the following raw materials in percentage by mass: 5% of vinyl-terminated silicone oil, 5% of modified nanoparticles, 3% of calcium stearate, 10102% of antioxidant, 3% of silicone curing agent, and the remainder is silicone matrix.

[0133] The nanoparticles are composed of nano silicon dioxide and nano aluminum oxide in a mass ratio of 4:1.

[0134] The preparation method of the nano-modified silicon dioxide is as follows:

[0135] The nano-silicon dioxide and nano-alumina are uniformly mixed in a mass ratio of 3:1.5, and then dried at 180° C. for 20 hours to obtain mixed nano-particles, and then 1.0 wt.% of a silane coupling agent and xylene 2.5 times the weight of the mixed nano-particles are added to the mixed nano-particles, and modified at 110° C. for 5 hours. After the modification is completed, the mixture is filtered, washed with acetone to remove unreacted nano-particles, and dried to obtain modified nano-particles;

[0136] The silane coupling agent is composed of silane coupling agent KH-560 and silane coupling agent KH-570 in a mass ratio of 1.5:4.5.

[0137] The preparation method of the injection molding silicone mold comprises the following steps:

[0138] S1. Weighing raw materials according to proportion to prepare modified nanoparticles;

[0139] S2, weighing raw materials according to proportion, and preparing outer layer raw materials and inner layer raw materials respectively;

[0140] S3, adding the outer layer raw material into the pressing mold, extruding and molding, pouring the inner layer raw material into the mold after the outer layer material is about to solidify (80% of the solidification time, the solidification time can be measured by experiment), and demoulding after solidification to obtain an injection molding silicone mold.

[0141] Example 6: An injection molding silicone mold, which comprises an inner layer and an outer layer from the inside to the outside. The thickness of the inner layer is 35% of the total thickness of the mold, and the thickness of the outer layer is 65% of the total thickness of the mold.

[0142] The outer layer is composed of the following raw materials in percentage by mass: 5% of vinyl-terminated silicone oil, 10102% of antioxidant, 3% of silicone curing agent, and the remainder is silicone matrix.

[0143] The inner layer is composed of the following raw materials in percentage by mass: 5% of vinyl-terminated silicone oil, 5% of modified nanoparticles, 3% of calcium stearate, 10102% of antioxidant, 3% of silicone curing agent, and the remainder is silicone matrix.

[0144] The nanoparticles are composed of nano silicon dioxide and nano aluminum oxide in a mass ratio of 4:1.

[0145] The preparation method of the nano-modified silicon dioxide is as follows:

[0146] The nano-silicon dioxide and nano-alumina are uniformly mixed in a mass ratio of 3:1.5, and then dried at 200° C. for 10 hours to obtain mixed nano-particles, and then 1.0 wt.% of a silane coupling agent and xylene 2.5 times the weight of the mixed nano-particles are added to the mixed nano-particles, and modified at 110° C. for 5 hours. After the modification is completed, the mixture is filtered, washed with acetone to remove unreacted nano-particles, and dried to obtain modified nano-particles;

[0147] The silane coupling agent is composed of silane coupling agent KH-560 and silane coupling agent KH-570 in a mass ratio of 1.5:4.5.

[0148] The preparation method of the injection molding silicone mold comprises the following steps:

[0149] S1. Weighing raw materials according to proportion to prepare modified nanoparticles;

[0150] S2, weighing raw materials according to proportion, and preparing outer layer raw materials and inner layer raw materials respectively;

[0151] S3, adding the outer layer raw material into the pressing mold, extruding and molding, pouring the inner layer raw material into the mold after the outer layer material is about to solidify (80% of the solidification time, the solidification time can be measured by experiment), and demoulding after solidification to obtain an injection molding silicone mold.

[0152] Example 7: An injection molding silicone mold, which comprises an inner layer and an outer layer from the inside to the outside, wherein the thickness of the inner layer is 35% of the total thickness of the mold, and the thickness of the outer layer is 65% of the total thickness of the mold.

[0153] The outer layer is composed of the following raw materials in percentage by mass: 5% of vinyl-terminated silicone oil, 10102% of antioxidant, 3% of silicone curing agent, and the remainder is silicone matrix.

[0154] The inner layer is composed of the following raw materials in percentage by mass: 5% of vinyl-terminated silicone oil, 5% of modified nanoparticles, 3% of calcium stearate, 10102% of antioxidant, 3% of silicone curing agent, and the remainder is silicone matrix.

[0155] The nanoparticles are composed of nano silicon dioxide and nano aluminum oxide in a mass ratio of 4:1.

[0156] The preparation method of the nano-modified silicon dioxide is as follows:

[0157] The nano-silicon dioxide and nano-alumina are uniformly mixed in a mass ratio of 3:1.5, and then dried at 185° C. for 15 hours to obtain mixed nano-particles, and then 0.5 wt.% of a silane coupling agent and xylene 2.5 times the weight of the mixed nano-particles are added to the mixed nano-particles, and modified at 110° C. for 5 hours. After the modification is completed, the mixture is filtered, washed with acetone to remove unreacted nano-particles, and dried to obtain modified nano-particles;

[0158] The silane coupling agent is composed of silane coupling agent KH-560 and silane coupling agent KH-570 in a mass ratio of 1.5:4.5.

[0159] The preparation method of the injection molding silicone mold comprises the following steps:

[0160] S1. Weighing raw materials according to proportion to prepare modified nanoparticles;

[0161] S2, weighing raw materials according to proportion, and preparing outer layer raw materials and inner layer raw materials respectively;

[0162] S3, adding the outer layer raw material into the pressing mold, extruding and molding, pouring the inner layer raw material into the mold after the outer layer material is about to solidify (80% of the solidification time, the solidification time can be measured by experiment), and demoulding after solidification to obtain an injection molding silicone mold.

[0163] Embodiment 8 is an injection molding silicone mold, which comprises an inner layer and an outer layer from the inside to the outside, wherein the thickness of the inner layer is 35% of the total thickness of the mold, and the thickness of the outer layer is 65% of the total thickness of the mold.

[0164] The outer layer is composed of the following raw materials in percentage by mass: 5% of vinyl-terminated silicone oil, 10102% of antioxidant, 3% of silicone curing agent, and the remainder is silicone matrix.

[0165] The inner layer is composed of the following raw materials in percentage by mass: 5% of vinyl-terminated silicone oil, 5% of modified nanoparticles, 3% of calcium stearate, 10102% of antioxidant, 3% of silicone curing agent, and the remainder is silicone matrix.

[0166] The nanoparticles are composed of nano silicon dioxide and nano aluminum oxide in a mass ratio of 4:1.

[0167] The preparation method of the nano-modified silicon dioxide is as follows:

[0168] The nano-silicon dioxide and nano-alumina are uniformly mixed in a mass ratio of 3:1.5, and then dried at 185° C. for 15 hours to obtain mixed nano-particles, and then 1.5 wt.% of a silane coupling agent and xylene 2.5 times the weight of the mixed nano-particles are added to the mixed nano-particles, and modified at 110° C. for 5 hours. After the modification is completed, the mixture is filtered, washed with acetone to remove unreacted nano-particles, and dried to obtain modified nano-particles;

[0169] The silane coupling agent is composed of silane coupling agent KH-560 and silane coupling agent KH-570 in a mass ratio of 1.5:4.5.

[0170] The preparation method of the injection molding silicone mold comprises the following steps:

[0171] S1. Weighing raw materials according to proportion to prepare modified nanoparticles;

[0172] S2, weighing raw materials according to proportion, and preparing outer layer raw materials and inner layer raw materials respectively;

[0173] S3, adding the outer layer raw material into the pressing mold, extruding and molding, pouring the inner layer raw material into the mold after the outer layer material is about to solidify (80% of the solidification time, the solidification time can be measured by experiment), and demoulding after solidification to obtain an injection molding silicone mold.

[0174] Example 9: An injection molding silicone mold, which comprises an inner layer and an outer layer from the inside to the outside. The thickness of the inner layer is 35% of the total thickness of the mold, and the thickness of the outer layer is 65% of the total thickness of the mold.

[0175] The outer layer is composed of the following raw materials in percentage by mass: 5% of vinyl-terminated silicone oil, 10102% of antioxidant, 3% of silicone curing agent, and the remainder is silicone matrix.

[0176] The inner layer is composed of the following raw materials in percentage by mass: 5% of vinyl-terminated silicone oil, 5% of modified nanoparticles, 3% of calcium stearate, 10102% of antioxidant, 3% of silicone curing agent, and the remainder is silicone matrix.

[0177] The nanoparticles are composed of nano silicon dioxide and nano aluminum oxide in a mass ratio of 4:1.

[0178] The preparation method of the nano-modified silicon dioxide is as follows:

[0179] The nano-silicon dioxide and nano-alumina are uniformly mixed in a mass ratio of 3:1.5, and then dried at 185° C. for 15 hours to obtain mixed nano-particles, and then 1.0 wt.% of a silane coupling agent and xylene twice the weight of the mixed nano-particles are added to the mixed nano-particles, and modified at 110° C. for 5 hours. After the modification is completed, the mixture is filtered, washed with acetone to remove unreacted nano-particles, and dried to obtain modified nano-particles;

[0180] The silane coupling agent is composed of silane coupling agent KH-560 and silane coupling agent KH-570 in a mass ratio of 1.5:4.5.

[0181] The preparation method of the injection molding silicone mold comprises the following steps:

[0182] S1. Weighing raw materials according to proportion to prepare modified nanoparticles;

[0183] S2, weighing raw materials according to proportion, and preparing outer layer raw materials and inner layer raw materials respectively;

[0184] S3, adding the outer layer raw material into the pressing mold, extruding and molding, pouring the inner layer raw material into the mold after the outer layer material is about to solidify (80% of the solidification time, the solidification time can be measured by experiment), and demoulding after solidification to obtain an injection molding silicone mold.

[0185] Embodiment 10 is an injection molding silicone mold, which comprises an inner layer and an outer layer from the inside to the outside, wherein the thickness of the inner layer is 35% of the total thickness of the mold, and the thickness of the outer layer is 65% of the total thickness of the mold.

[0186] The outer layer is composed of the following raw materials in percentage by mass: 5% of vinyl-terminated silicone oil, 10102% of antioxidant, 3% of silicone curing agent, and the remainder is silicone matrix.

[0187] The inner layer is composed of the following raw materials in percentage by mass: 5% of vinyl-terminated silicone oil, 5% of modified nanoparticles, 3% of calcium stearate, 10102% of antioxidant, 3% of silicone curing agent, and the remainder is silicone matrix.

[0188] The nanoparticles are composed of nano silicon dioxide and nano aluminum oxide in a mass ratio of 4:1.

[0189] The preparation method of the nano-modified silicon dioxide is as follows:

[0190] The nano-silicon dioxide and nano-alumina are uniformly mixed in a mass ratio of 3:1.5, and then dried at 185° C. for 15 hours to obtain mixed nano-particles, and then 1.0 wt.% of a silane coupling agent and xylene 3 times the weight of the mixed nano-particles are added to the mixed nano-particles, and modified at 110° C. for 5 hours. After the modification is completed, the mixture is filtered, washed with acetone to remove unreacted nano-particles, and dried to obtain modified nano-particles;

[0191] The silane coupling agent is composed of silane coupling agent KH-560 and silane coupling agent KH-570 in a mass ratio of 1.5:4.5.

[0192] The preparation method of the injection molding silicone mold comprises the following steps:

[0193] S1. Weighing raw materials according to proportion to prepare modified nanoparticles;

[0194] S2, weighing raw materials according to proportion, and preparing outer layer raw materials and inner layer raw materials respectively;

[0195] S3, adding the outer layer raw material into the pressing mold, extruding and molding, pouring the inner layer raw material into the mold after the outer layer material is about to solidify (80% of the solidification time, the solidification time can be measured by experiment), and demoulding after solidification to obtain an injection molding silicone mold.

[0196] Embodiment 11 is an injection molding silicone mold, which comprises an inner layer and an outer layer from the inside to the outside, wherein the thickness of the inner layer is 35% of the total thickness of the mold, and the thickness of the outer layer is 65% of the total thickness of the mold.

[0197] The outer layer is composed of the following raw materials in percentage by mass: 5% of vinyl-terminated silicone oil, 10102% of antioxidant, 3% of silicone curing agent, and the remainder is silicone matrix.

[0198] The inner layer is composed of the following raw materials in percentage by mass: 5% of vinyl-terminated silicone oil, 5% of modified nanoparticles, 3% of calcium stearate, 10102% of antioxidant, 3% of silicone curing agent, and the remainder is silicone matrix.

[0199] The nanoparticles are composed of nano silicon dioxide and nano aluminum oxide in a mass ratio of 4:1.

[0200] The preparation method of the nano-modified silicon dioxide is as follows:

[0201] The nano-silicon dioxide and nano-alumina are mixed uniformly in a mass ratio of 3:1.5, and then dried at 185° C. for 15 hours to obtain mixed nano-particles, and then 1.0 wt.% of a silane coupling agent and xylene 2.5 times the weight of the mixed nano-particles are added to the mixed nano-particles, and modified at 100° C. for 7 hours. After the modification is completed, the mixture is filtered, washed with acetone to remove unreacted nano-particles, and dried to obtain modified nano-particles;

[0202] The silane coupling agent is composed of silane coupling agent KH-560 and silane coupling agent KH-570 in a mass ratio of 1.5:4.5.

[0203] The preparation method of the injection molding silicone mold comprises the following steps:

[0204] S1. Weighing raw materials according to proportion to prepare modified nanoparticles;

[0205] S2, weighing raw materials according to proportion, and preparing outer layer raw materials and inner layer raw materials respectively;

[0206] S3, adding the outer layer raw material into the pressing mold, extruding and molding, pouring the inner layer raw material into the mold after the outer layer material is about to solidify (80% of the solidification time, the solidification time can be measured by experiment), and demoulding after solidification to obtain an injection molding silicone mold.

[0207] Example 12: An injection molding silicone mold, which comprises an inner layer and an outer layer from the inside to the outside, wherein the thickness of the inner layer is 35% of the total thickness of the mold, and the thickness of the outer layer is 65% of the total thickness of the mold.

[0208] The outer layer is composed of the following raw materials in percentage by mass: 5% of vinyl-terminated silicone oil, 10102% of antioxidant, 3% of silicone curing agent, and the remainder is silicone matrix.

[0209] The inner layer is composed of the following raw materials in percentage by mass: 5% of vinyl-terminated silicone oil, 5% of modified nanoparticles, 3% of calcium stearate, 10102% of antioxidant, 3% of silicone curing agent, and the remainder is silicone matrix.

[0210] The nanoparticles are composed of nano silicon dioxide and nano aluminum oxide in a mass ratio of 4:1.

[0211] The preparation method of the nano-modified silicon dioxide is as follows:

[0212] The nano-silicon dioxide and nano-alumina are uniformly mixed in a mass ratio of 3:1.5, and then dried at 185° C. for 15 hours to obtain mixed nano-particles, and then 1.0 wt.% of a silane coupling agent and xylene 2.5 times the weight of the mixed nano-particles are added to the mixed nano-particles, and modified at 120° C. for 3 hours. After the modification is completed, the mixture is filtered, washed with acetone to remove unreacted nano-particles, and dried to obtain modified nano-particles;

[0213] The silane coupling agent is composed of silane coupling agent KH-560 and silane coupling agent KH-570 in a mass ratio of 1.5:4.5.

[0214] The preparation method of the injection molding silicone mold comprises the following steps:

[0215] S1. Weighing raw materials according to proportion to prepare modified nanoparticles;

[0216] S2, weighing raw materials according to proportion, and preparing outer layer raw materials and inner layer raw materials respectively;

[0217] S3, adding the outer layer raw material into the pressing mold, extruding and molding, pouring the inner layer raw material into the mold after the outer layer material is about to solidify (80% of the solidification time, the solidification time can be measured by experiment), and demoulding after solidification to obtain an injection molding silicone mold.

[0218] Example 13: An injection molding silicone mold, which comprises an inner layer and an outer layer from the inside to the outside, wherein the thickness of the inner layer is 35% of the total thickness of the mold, and the thickness of the outer layer is 65% of the total thickness of the mold.

[0219] The outer layer is composed of the following raw materials in percentage by mass: 5% of vinyl-terminated silicone oil, 10102% of antioxidant, 3% of silicone curing agent, and the remainder is silicone matrix.

[0220] The inner layer is composed of the following raw materials in percentage by mass: 5% of vinyl-terminated silicone oil, 5% of modified nanoparticles, 3% of calcium stearate, 10102% of antioxidant, 3% of silicone curing agent, and the remainder is silicone matrix.

[0221] The nanoparticles are composed of nano silicon dioxide and nano aluminum oxide in a mass ratio of 4:1.

[0222] The preparation method of the nano-modified silicon dioxide is as follows:

[0223] The nano-silicon dioxide and nano-alumina are uniformly mixed in a mass ratio of 3:1.5, and then dried at 185° C. for 15 hours to obtain mixed nano-particles, and then 1.0 wt.% of a silane coupling agent and xylene 2.5 times the weight of the mixed nano-particles are added to the mixed nano-particles, and modified at 110° C. for 5 hours. After the modification is completed, the mixture is filtered, washed with acetone to remove unreacted nano-particles, and dried to obtain modified nano-particles;

[0224] The silane coupling agent is composed of silane coupling agent KH-560 and silane coupling agent KH-570 in a mass ratio of 1:4.

[0225] The preparation method of the injection molding silicone mold comprises the following steps:

[0226] S1. Weighing raw materials according to proportion to prepare modified nanoparticles;

[0227] S2, weighing raw materials according to proportion, and preparing outer layer raw materials and inner layer raw materials respectively;

[0228] S3, adding the outer layer raw material into the pressing mold, extruding and molding, pouring the inner layer raw material into the mold after the outer layer material is about to solidify (80% of the solidification time, the solidification time can be measured by experiment), and demoulding after solidification to obtain an injection molding silicone mold.

[0229] Example 14: An injection molding silicone mold, which comprises an inner layer and an outer layer from the inside to the outside, wherein the thickness of the inner layer is 35% of the total thickness of the mold, and the thickness of the outer layer is 65% of the total thickness of the mold.

[0230] The outer layer is composed of the following raw materials in percentage by mass: 5% of vinyl-terminated silicone oil, 10102% of antioxidant, 3% of silicone curing agent, and the remainder is silicone matrix.

[0231] The inner layer is composed of the following raw materials in percentage by mass: 5% of vinyl-terminated silicone oil, 5% of modified nanoparticles, 3% of calcium stearate, 10102% of antioxidant, 3% of silicone curing agent, and the remainder is silicone matrix.

[0232] The nanoparticles are composed of nano silicon dioxide and nano aluminum oxide in a mass ratio of 4:1.

[0233] The preparation method of the nano-modified silicon dioxide is as follows:

[0234] The nano-silicon dioxide and nano-alumina are uniformly mixed in a mass ratio of 3:1.5, and then dried at 185° C. for 15 hours to obtain mixed nano-particles, and then 1.0 wt.% of a silane coupling agent and xylene 2.5 times the weight of the mixed nano-particles are added to the mixed nano-particles, and modified at 110° C. for 5 hours. After the modification is completed, the mixture is filtered, washed with acetone to remove unreacted nano-particles, and dried to obtain modified nano-particles;

[0235] The silane coupling agent is composed of silane coupling agent KH-560 and silane coupling agent KH-570 in a mass ratio of 2:5.

[0236] The preparation method of the injection molding silicone mold comprises the following steps:

[0237] S1. Weighing raw materials according to proportion to prepare modified nanoparticles;

[0238] S2, weighing raw materials according to proportion, and preparing outer layer raw materials and inner layer raw materials respectively;

[0239] S3, adding the outer layer raw material into the pressing mold, extruding and molding, pouring the inner layer raw material into the mold after the outer layer material is about to solidify (80% of the solidification time, the solidification time can be measured by experiment), and demoulding after solidification to obtain an injection molding silicone mold.

[0240] After testing, the number of times the molds of Examples 4-14 are used and the effects of use are not significantly different from those of Examples 1-3.

[0241] The principles and implementation methods of the present invention are described in this article using specific examples. The description of the above embodiments is only used to help understand the method and core idea of ​​the present invention. At the same time, for those skilled in the art, according to the idea of ​​the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A gel injection molding silicone mold, characterized in that: From inside to outside, there are an inner layer and an outer layer, the thickness of the inner layer is 20% to 50% of the total thickness of the mold, and the thickness of the outer layer is 50% to 80% of the total thickness of the mold; The outer layer is composed of the following raw materials in percentage by mass: 4-10% vinyl-terminated silicone oil, 1-2% antioxidant, 1-3% curing agent, and the remainder is a silicone matrix; The inner layer is composed of the following raw materials in percentage by mass: 4-10% of vinyl-terminated silicone oil, 1-10% of modified nanoparticles, 1-3% of calcium stearate, 1-2% of antioxidant, 1-3% of curing agent, and the remainder is a silica gel matrix; The preparation method of the modified nanoparticles is as follows: The nano-silicon dioxide and nano-aluminum oxide are mixed uniformly in proportion and then dried to obtain mixed nano-particles, and then a silane coupling agent and xylene are added to the mixed nano-particles for modification, and after the modification is completed, the mixture is filtered, washed, and dried to obtain modified nano-particles; The mass ratio of the nano silicon dioxide to the nano aluminum oxide is (3-5):(0.5-1.5).

2. The gel injection molding silicone mold according to claim 1, characterized in that: The nanoparticles are composed of nano silicon dioxide and nano aluminum oxide in a mass ratio of 4:

1.

3. The gel injection molding silicone mold according to claim 1, characterized in that: The drying temperature of the mixed nanoparticles is 180° C. to 200° C., and the drying time is 10 to 20 hours.

4. The gel injection molding silicone mold according to claim 1, characterized in that: The added amount of the silane coupling agent is 0.5wt.% to 1.5wt.% of the mixed nanoparticles.

5. The gel injection molding silicone mold according to claim 4, characterized in that: The added amount of the silane coupling agent is 1.0 wt.% of the mixed nanoparticles.

6. The gel injection molding silicone mold according to claim 1, characterized in that: The mass ratio of the mixed nanoparticles to the xylene is 1:(0.5-5).

7. The gel injection molding silicone mold according to claim 1, characterized in that: The modification temperature is 100° C. to 120° C., and the modification time is 3 to 7 hours.

8. The gel injection molding silicone mold according to claim 7, characterized in that: The modification temperature is 110° C. and the modification time is 5 hours.

9. The gel injection molding silicone mold according to claim 1, characterized in that: The silane coupling agents are silane coupling agent KH-560 and silane coupling agent KH-570, and the mass ratio of the silane coupling agent KH-560 to the silane coupling agent KH-570 is (1-2):(4-5).

10. The method for preparing the gel injection molding silicone mold according to any one of claims 1 to 9, comprising the following steps: S1. Weighing raw materials according to proportion to prepare modified nanoparticles; S2, weighing raw materials according to proportion, and preparing outer layer raw materials and inner layer raw materials respectively; S3, adding the outer layer raw material into the pressing mold, extruding and molding, pouring the inner layer raw material into the mold after the outer layer material is about to solidify, and demoulding after solidification to obtain an injection molding silicone mold.

Citation Information

Patent Citations

  • Method for rapidly manufacturing low-temperature alloy pouring mould by high-temperature resistant silicon rubber

    CN102773408A

  • Preparation method of precision SiC ceramic formed by gel casting based on silicone mold and precision SiC ceramic

    CN106747457A

  • Viscoelastic magnetic grinding tool with silicone rubber as matrix and preparation method thereof

    CN107932348A

  • Elastic mold

    JP1993057730A