High-temperature-resistant high-strength wear-resistant liquid silica gel and preparation method thereof
Through specific proportional materials and process treatments, the wear resistance and high-temperature performance of liquid silicone is improved, and the problem of short service life of existing liquid silicone in high-temperature environments is solved, extending service life and reducing resource waste.
Patent Information
- Application Number
- CN202411247156.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-12-06
AI Technical Summary
The existing liquid silicone has a short service life and poor wear resistance in high temperature environments, resulting in frequent replacement and waste of resources.
Materials with specific ratios such as end vinyl silicone oil, polyvinyl silicone oil, vinyl silicone resin, gas phase white carbon black, silicon carbide, hexamethyldisilazane, methyl trimethoxysilane, end hydrogen-containing silicone oil, The surface of hydrogen-containing silicone oil, platinum catalyst and cerium isocyanate are modified by vacuum kneading and high-temperature treatment to improve the wear resistance of silicone.
It significantly improves the wear resistance and tensile strength of liquid silicone, extends its service life at high temperatures, reduces the number of gloves replaced, and avoids waste of resources.
Smart Images

Figure CN119081415A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of silicone gloves, and specifically relates to high-temperature resistant, high-strength, and wear-resistant liquid silicone and a preparation method thereof. Background Art
[0002] Liquid silicone, also known as liquid silicone, is a liquid rubber relative to solid high-temperature vulcanized silicone rubber. Liquid silicone is a highly active adsorption material and an amorphous substance. It is insoluble in water and any solvent, non-toxic and odorless, and has stable chemical properties. The ordinary liquid silicone on the market has the disadvantages of low strength, poor tearing, and very poor wear resistance. The liquid silicone gloves made have a very short service life and need to be replaced frequently, especially in some high-temperature occasions. The service life is even shorter and the gloves need to be replaced many times, resulting in a waste of resources. In this regard, we propose a high-temperature resistant, high-strength, and wear-resistant liquid silicone and a preparation method thereof. Summary of the invention
[0003] In view of the deficiencies in the prior art, the present invention provides a high-temperature resistant, high-strength, and wear-resistant liquid silicone and a preparation method thereof to solve the above technical problems.
[0004] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a high-temperature resistant, high-strength and wear-resistant liquid silicone, which is prepared from the following materials: 10-25 parts of terminal vinyl silicone oil, 2-10 parts of polyvinyl silicone oil, 10-25 parts of vinyl silicone resin, 0.5-2 parts of phenyl silicone oil, 20-30 parts of fumed silica, 5-15 parts of silicon carbide, 1-3 parts of hexamethyldisilazane, 1-3 parts of methyltrimethoxysilane, 5-10 parts of terminal hydrogen-containing silicone oil, 3-6 parts of side hydrogen-containing silicone oil, 0.1-0.5 parts of platinum catalyst, 0.005-0.1 parts of acetylene cyclohexanol and 0.5-3 parts of cerium isozincate.
[0005] The present application modifies the surface of fumed silica and silicon carbide by compounding hexamethyldisilazane and methyltrimethoxysilane, thereby making the surface of the inorganic filler organic and improving the compatibility with silicone oil. The treated silicon carbide also greatly improves the wear resistance of silica gel.
[0006] Preferably, the liquid silica gel is prepared from the following materials: 10 parts of terminal vinyl silicone oil, 8 parts of polyvinyl silicone oil, 12 parts of vinyl silicone resin, 0.5 parts of phenyl silicone oil, 22 parts of fumed silica, 8 parts of silicon carbide, 2 parts of hexamethyldisilazane, 2 parts of methyltrimethoxysilane, 6 parts of terminal hydrogen-containing silicone oil, 5 parts of side hydrogen-containing silicone oil, 0.5 parts of platinum catalyst, 0.01 parts of acetylene cyclohexanol and 2.5 parts of cerium isozincate.
[0007] Preferably, the viscosity of the vinyl-terminated silicone oil is 10000cps-80000cps, and the vinyl content is 0.1%-1%, the viscosity of the polyvinyl silicone oil is 10000cps-60000cps, and the vinyl content is 2%-10%, the viscosity of the vinyl silicone resin is 5000cps-50000cps, and the vinyl content is 1%-5%, the viscosity of the phenyl silicone oil is 100cps-1000cps, and the phenyl content is 3%-10%, and the specific surface area of the fumed silica is 300m 2 / g-400m 2 / g, the particle size of silicon carbide is 300 mesh-2000 mesh, the hydrogen content of the end hydrogen-containing silicone oil is 0.05%-0.2%, and the hydrogen content of the side hydrogen-containing silicone oil is 0.1%-0.5%.
[0008] A method for preparing high temperature resistant, high strength and wear resistant liquid silicone, the preparation steps are:
[0009] S1. Prepare the following materials: 10-25 parts of vinyl-terminated silicone oil, 2-10 parts of polyvinyl silicone oil, 10-25 parts of vinyl silicone resin, 0.5-2 parts of phenyl silicone oil, 20-30 parts of fumed silica, 5-15 parts of silicon carbide, 1-3 parts of hexamethyldisilazane, 1-3 parts of methyltrimethoxysilane, 5-10 parts of terminal hydrogen-containing silicone oil, 3-6 parts of side hydrogen-containing silicone oil, 0.1-0.5 parts of platinum catalyst, 0.005-0.1 parts of acetylene cyclohexanol and 0.5-3 parts of cerium isozincate;
[0010] S2, put the vinyl-terminated silicone oil, polyvinyl silicone oil, vinyl silicone resin, hexamethyldisilazane and methyltrimethoxysilane into a vacuum kneader according to the proportion, and stir and knead for 20-30 minutes;
[0011] S3, add fumed silica and silicon carbide into the kneader in 4-6 times according to the ratio, after adding, turn on the cooling water, and cold refine for 2-4 hours;
[0012] S4. Turn on the vacuum pump, adjust the vacuum degree in the kneader to -0.1MPa, and continue to stir the material under vacuum conditions of 160℃-180℃ for 2-4h;
[0013] S5. Stop vacuuming, open the vent valve, turn off the steam, turn on the cooling water, cool the material, and discharge the material after the material cools to below 50°C to obtain a wear-resistant liquid silicone base material;
[0014] S6, transfer the wear-resistant liquid silicone base material into a special material tank of a vacuum high-speed mixer for standby use, and proceed to the next step of preparation;
[0015] Phenyl silicone oil, terminal hydrogen silicone oil, side hydrogen silicone oil, acetylene cyclohexanol and cerium isozincate are added to the wear-resistant liquid silicone base material, and the mixture is vacuum stirred for 1-2 hours and then filtered and packaged with a 100-200 mesh filter to complete the preparation of the wear-resistant liquid silicone component A;
[0016] S7, wear-resistant liquid silica gel B component, 5000ppm platinum catalyst;
[0017] S8. Mix and stir the A and B component materials in a ratio of 100:0.3, pour the mixture into a mold for making a test piece, and then process it on a flat vulcanizer with a pressure of 13MPa, a temperature of 150°C and a curing time of 10min. After curing, a silicone test piece with good wear resistance can be obtained, and various physical properties can be tested.
[0018] Preferably, in step S2, the terminal vinyl silicone oil, polyvinyl silicone oil, vinyl silicone resin, hexamethyldisilazane and methyltrimethoxysilane are put into the vacuum kneader at one time, and stirring is started. During the stirring process, the preparation personnel closely observe the vacuum kneader and wait for the stirring and kneading to be completed;
[0019] The present invention adds a small amount of phenyl silicone oil, which will slowly and continuously seep out from the silicone product, increasing the lubricity of the silicone surface, thereby improving the wear resistance of the silicone product;
[0020] The use of cerium isozincate effectively improves the temperature resistance of silica gel. The temperature resistance of ordinary silica gel is 200-230 degrees, while the temperature resistance of the silica gel of the present invention can reach 280-300 degrees, which greatly increases the service life of silica gel in high temperature occasions. At the same high temperature, the product has more excellent mechanical properties, thereby also improving the wear resistance of silica gel products at high temperatures;
[0021] The end-hydrogen silicone oil and the side-hydrogen silicone oil are added in a specific ratio, so that the end-vinyl silicone oil, polyvinyl silicone oil and vinyl silicone resin are chain extended during cross-linking, thereby improving the tensile strength and tearing properties of the silicone.
[0022] The use of polyvinyl silicone and vinyl silicone resin in combination with short vinyl silicone oil increases the centralized cross-linking degree of silicone, making the surface smoother after silicone curing, and also improves the wear resistance of the products after silicone curing.
[0023] Preferably, in step S3, after the stirring and kneading is completed, the fumed silica and silicon carbide are added successively according to the ratio, and stirring is performed during each addition process. After the addition is completed, the feed port of the kneader is closed and the cold refining operation is performed.
[0024] The present application ensures that these additives are evenly dispersed in the mixture by adding fumed silica and silicon carbide in succession and stirring after each addition. This dispersion uniformity is crucial to the performance of the final product because it can avoid uneven performance caused by local excessively high or low concentrations. The stirring operation helps to accelerate the mixing of the components in the mixture, allowing the fumed silica and silicon carbide to be integrated into the matrix more quickly, thereby improving the mixing efficiency.
[0025] Preferably, after the preliminary mixing and kneading is completed in step S4, the air and other non-condensable gases in the kneader are evacuated by a vacuum pump, and the temperature is adjusted so that the internal structure of the material changes under the dual effects of high temperature and vacuum.
[0026] Under the dual effects of high temperature and vacuum, the molecular structure and arrangement of the material may change, thereby improving its physical properties. For example, the hardness, strength, toughness and other properties of the material may be improved to meet higher usage requirements; after removing impurities and gases, the uniformity and consistency of the material are improved, which helps to reduce defects and defective product rates in the product.
[0027] Preferably, in step S5, when the predetermined stirring time and heat treatment effect are achieved, the equipment is turned off, the vacuum degree in the kneader is slowly released to a normal pressure state, and the heat of the material and the inside of the equipment is taken away by cooling water.
[0028] The slow release of vacuum in this application can avoid the impact of sudden exposure of materials to normal pressure environment, reduce the damage to material structure and changes in performance, and remove the heat from materials and equipment through cooling water, which can effectively prevent overheating damage caused by long-term high-temperature operation of materials and equipment, optimize the production process, and reduce waste and losses.
[0029] Preferably, an electronic scale is used to proportion the materials in step S8.
[0030] Preferably, in step S6, the uniformly stirred material is slowly poured into a filter press, and pressure is applied to allow the material to pass through the filter screen to achieve solid-liquid separation.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] The present application improves the wear resistance of silicone by compounding and combining different materials, greatly increases the service life of silicone in high temperature environments, improves the wear resistance of silicone products at high temperatures, improves the tensile strength and tearing properties of silicone, reduces the number of times gloves need to be replaced, and avoids excessive waste of resources. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is a framework diagram of the preparation steps of the present invention. DETAILED DESCRIPTION
[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] Example 1
[0036] A method for preparing high temperature resistant, high strength and wear resistant liquid silicone, the preparation steps are:
[0037] S1. Prepare the following materials: 10 parts of vinyl-terminated silicone oil, 8 parts of polyvinyl silicone oil, 12 parts of vinyl silicone resin, 0.5 parts of phenyl silicone oil, 22 parts of fumed silica, 8 parts of silicon carbide, 2 parts of hexamethyldisilazane, 2 parts of methyltrimethoxysilane, 6 parts of terminal hydrogen-containing silicone oil, 5 parts of side hydrogen-containing silicone oil, 0.5 parts of platinum catalyst, 0.01 parts of acetylene cyclohexanol and 2.5 parts of cerium isozincate;
[0038] S2, put the vinyl-terminated silicone oil, polyvinyl silicone oil, vinyl silicone resin, hexamethyldisilazane and methyltrimethoxysilane into a vacuum kneader according to the proportion, and stir and knead for 30 minutes;
[0039] S3, add fumed silica and silicon carbide into the kneader in 4 times according to the ratio. After adding, turn on the cooling water and cold refine for 2 hours;
[0040] S4. Turn on the vacuum pump, adjust the vacuum degree in the kneader to -0.1 MPa, and continue stirring the material under vacuum conditions at 160°C for 2 hours;
[0041] S5. Stop vacuuming, open the vent valve, turn off the steam, turn on the cooling water, cool the material, and discharge the material after the material cools to below 50°C to obtain a wear-resistant liquid silicone base material;
[0042] S6, transfer the wear-resistant liquid silicone base material into a special material tank of a vacuum high-speed mixer for standby use, and proceed to the next step of preparation;
[0043] Phenyl silicone oil, terminal hydrogen silicone oil, side hydrogen silicone oil, acetylene cyclohexanol and cerium isozincate were added to the wear-resistant liquid silicone base material, and the mixture was vacuum stirred for 2 hours and then filtered and packaged with a 100-mesh filter to complete the preparation of the wear-resistant liquid silicone component A;
[0044] S7, wear-resistant liquid silica gel B component, 5000ppm platinum catalyst;
[0045] S8. Mix and stir the A and B component materials in a ratio of 100:0.3, pour the mixture into a mold for making a test piece, and then process it on a flat vulcanizer with a pressure of 13MPa, a temperature of 150°C and a curing time of 10min. After curing, a silicone test piece with good wear resistance can be obtained, and various physical properties can be tested.
[0046] Example 2
[0047] A method for preparing high temperature resistant, high strength and wear resistant liquid silicone, the preparation steps are:
[0048] S1. Prepare the following materials: 15 parts of vinyl-terminated silicone oil, 8 parts of polyvinyl silicone oil, 12 parts of vinyl silicone resin, 1 part of phenyl silicone oil, 22 parts of fumed silica, 6 parts of silicon carbide, 1 part of hexamethyldisilazane, 2 parts of methyltrimethoxysilane, 6 parts of hydrogen-terminated silicone oil, 5 parts of hydrogen-terminated silicone oil, 0.1 parts of platinum catalyst, 0.1 parts of acetylene cyclohexanol and 0.5 parts of cerium isozincate;
[0049] S2, put the vinyl-terminated silicone oil, polyvinyl silicone oil, vinyl silicone resin, hexamethyldisilazane and methyltrimethoxysilane into a vacuum kneader according to the proportion, and stir and knead for 20 minutes;
[0050] S3, add fumed silica and silicon carbide into the kneader in 5 times according to the ratio. After adding, turn on the cooling water and cold refine for 3 hours;
[0051] S4. Turn on the vacuum pump, adjust the vacuum degree in the kneader to -0.1 MPa, and continue stirring the material under vacuum conditions at 150°C for 3 hours;
[0052] S5. Stop vacuuming, open the vent valve, turn off the steam, turn on the cooling water, cool the material, and discharge the material after the material cools to below 50°C to obtain a wear-resistant liquid silicone base material;
[0053] S6, transfer the wear-resistant liquid silicone base material into a special material tank of a vacuum high-speed mixer for standby use, and proceed to the next step of preparation;
[0054] Phenyl silicone oil, terminal hydrogen silicone oil, side hydrogen silicone oil, acetylene cyclohexanol and cerium isozincate were added to the wear-resistant liquid silicone base material, and the mixture was vacuum stirred for 1 hour and then filtered and packaged with a 200-mesh filter to complete the preparation of the wear-resistant liquid silicone component A;
[0055] S7, wear-resistant liquid silica gel B component, 5000ppm platinum catalyst;
[0056] S8. Mix and stir the A and B component materials in a ratio of 100:0.3, pour the mixture into a mold for making a test piece, and then process it on a flat vulcanizer with a pressure of 13MPa, a temperature of 150°C and a curing time of 10min. After curing, a silicone test piece with good wear resistance can be obtained, and various physical properties can be tested.
[0057] Example 3
[0058] A method for preparing high temperature resistant, high strength and wear resistant liquid silicone, the preparation steps are:
[0059] S1. Prepare the following materials: 10 parts of vinyl-terminated silicone oil, 9 parts of polyvinyl silicone oil, 19 parts of vinyl silicone resin, 1.5 parts of phenyl silicone oil, 25 parts of fumed silica, 8 parts of silicon carbide, 1.5 parts of hexamethyldisilazane, 1.5 parts of methyltrimethoxysilane, 8 parts of terminal hydrogen-containing silicone oil, 5 parts of side hydrogen-containing silicone oil, 0.5 parts of platinum catalyst, 0.1 parts of acetylene cyclohexanol and 1.6 parts of cerium isozincate;
[0060] S2, put the vinyl-terminated silicone oil, polyvinyl silicone oil, vinyl silicone resin, hexamethyldisilazane and methyltrimethoxysilane into a vacuum kneader according to the proportion, and stir and knead for 22 minutes;
[0061] S3, add fumed silica and silicon carbide into the kneader in 6 times according to the ratio. After adding, turn on the cooling water and cold refine for 3 hours;
[0062] S4. Turn on the vacuum pump, adjust the vacuum degree in the kneader to -0.1 MPa, and continue stirring the material under vacuum conditions at 160°C for 2 hours;
[0063] S5. Stop vacuuming, open the vent valve, turn off the steam, turn on the cooling water, cool the material, and discharge the material after the material cools to below 50°C to obtain a wear-resistant liquid silicone base material;
[0064] S6, transfer the wear-resistant liquid silicone base material into a special material tank of a vacuum high-speed mixer for standby use, and proceed to the next step of preparation;
[0065] Phenyl silicone oil, terminal hydrogen silicone oil, side hydrogen silicone oil, acetylene cyclohexanol and cerium isozincate were added to the wear-resistant liquid silicone base material, and the mixture was vacuum stirred for 1 hour and then filtered and packaged with a 150-mesh filter to complete the preparation of the wear-resistant liquid silicone component A;
[0066] S7, wear-resistant liquid silica gel B component, 5000ppm platinum catalyst;
[0067] S8. Mix and stir the A and B component materials in a ratio of 100:0.3, pour the mixture into a mold for making a test piece, and then process it on a flat vulcanizer with a pressure of 13MPa, a temperature of 150°C and a curing time of 10min. After curing, a silicone test piece with good wear resistance can be obtained, and various physical properties can be tested.
[0068] Comparative Example 1
[0069] The preparation steps of liquid silicone are as follows:
[0070] A1. Prepare raw materials: silane (purity must reach more than 99%), sodium hydroxide, ethylene glycol, isopropanol, water, fillers, additives, masterbatches and additives;
[0071] A2. Select a clean reactor to ensure that there are no impurities and residues. Slowly add silane into the reactor. While maintaining the temperature in the reactor at a suitable level, add sodium hydroxide and water in sequence. After the reaction is completed, add ethylene glycol and isopropanol.
[0072] A3, the mixed raw materials react, and during the reaction process, the temperature in the reactor is maintained within a suitable range;
[0073] A4. After the reaction is completed, the mixture is evaporated by heating and pressurizing to remove the water therein. As the water evaporates, the mixture gradually forms a dense liquid silica gel;
[0074] A5. Carry out finished product inspection on the liquid silicone and check whether the appearance of the liquid silicone is uniform and free of impurities, bubbles and other defects.
[0075] The liquid silicone prepared in Comparative Example 1 has low strength, poor tearing and very poor wear resistance. The liquid silicone gloves made from it have a very short service life and need to be replaced frequently. The liquid silicone prepared in the embodiment improves the wear resistance of silicone by compounding different materials, greatly increases the service life of silicone in high temperature environments, improves the wear resistance of silicone products at high temperatures, improves the tensile strength and tearing properties of silicone, reduces the number of times gloves are replaced, and avoids excessive waste of resources.
[0076] The specific proportions of the formula of the present invention when used, the national standards used in testing the product, the methods for performing performance testing, and the data obtained from testing the product during the research and development process.
[0077] Table 1 below shows the properties of the prepared liquid silica gel.
[0078]
[0079] Table 1
[0080] Table 2 below is a table showing the physical properties of the silica gel test pieces prepared in different embodiments and comparative examples.
[0081]
[0082]
[0083] Table 2
[0084] Density detection
[0085] Density testing is carried out based on HG / T2728-2012 standard;
[0086] Hardness testing
[0087] The hardness test is carried out based on GB / T531-2008 standard;
[0088] Tensile strength test
[0089] The tensile strength test is carried out based on GB / T528-2009 standard;
[0090] Tear strength test
[0091] The tear strength test is carried out based on GB / T529-2008 standard;
[0092] Wear index test
[0093] The wear index test is implemented based on GB / T1689-2014 standard;
[0094] High temperature resistance test
[0095] The detection steps are:
[0096] A1. Select representative liquid silicone samples to ensure that the sample quality meets the test requirements and has no obvious defects or contamination. Perform necessary pretreatment on the samples, such as cleaning and drying, to ensure the accuracy of the test results.
[0097] A2. Place the treated liquid silicone sample in the testing instrument to ensure that the sample is heated evenly;
[0098] A3. Set the test instrument parameters, start the test instrument, conduct the test, regularly observe the appearance and morphology of the silica gel samples, and record the relevant data;
[0099] A4. Record various data during the test, including test temperature, time, and sample changes;
[0100] A5. Based on the recorded data and observed phenomena, analyze the high temperature resistance of liquid silicone and evaluate its stability, durability and possible physical or chemical changes at high temperatures.
[0101] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0102] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A high temperature resistant, high strength and wear resistant liquid silicone, characterized in that: Liquid silica gel is prepared from the following materials: 10-25 parts of terminal vinyl silicone oil, 2-10 parts of polyvinyl silicone oil, 10-25 parts of vinyl silicone resin, 0.5-2 parts of phenyl silicone oil, 20-30 parts of fumed silica, 5-15 parts of silicon carbide, 1-3 parts of hexamethyldisilazane, 1-3 parts of methyltrimethoxysilane, 5-10 parts of terminal hydrogen-containing silicone oil, 3-6 parts of side hydrogen-containing silicone oil, 0.1-0.5 parts of platinum catalyst, 0.005-0.1 parts of acetylene cyclohexanol and 0.5-3 parts of cerium isozincate.
2. The high temperature resistant, high strength and wear resistant liquid silicone according to claim 1, characterized in that: Liquid silica gel is specifically prepared from the following materials: 10 parts of terminal vinyl silicone oil, 8 parts of polyvinyl silicone oil, 12 parts of vinyl silicone resin, 0.5 parts of phenyl silicone oil, 22 parts of fumed silica, 8 parts of silicon carbide, 2 parts of hexamethyldisilazane, 2 parts of methyltrimethoxysilane, 6 parts of terminal hydrogen-containing silicone oil, 5 parts of side hydrogen-containing silicone oil, 0.5 parts of platinum catalyst, 0.01 parts of acetylene cyclohexanol and 2.5 parts of cerium isozincate.
3. The high temperature resistant, high strength and wear resistant liquid silicone according to claim 1, characterized in that: The viscosity of vinyl-terminated silicone oil is 10000cps-80000cps, and the vinyl content is 0.1%-1%. The viscosity of polyvinyl silicone oil is 10000cps-60000cps, and the vinyl content is 2%-10%. The viscosity of vinyl silicone resin is 5000cps-50000cps, and the vinyl content is 1%-5%. The viscosity of phenyl silicone oil is 100cps-1000cps, and the phenyl content is 3%-10%. The specific surface area of fumed silica is 300m 2 / g-400m 2 / g, the particle size of silicon carbide is 300 mesh-2000 mesh, the hydrogen content of the end hydrogen-containing silicone oil is 0.05%-0.2%, and the hydrogen content of the side hydrogen-containing silicone oil is 0.1%-0.5%.
4. A method for preparing high temperature resistant, high strength and wear resistant liquid silicone, characterized in that: The preparation steps are: S1. Prepare the following materials: 10-25 parts of vinyl-terminated silicone oil, 2-10 parts of polyvinyl silicone oil, 10-25 parts of vinyl silicone resin, 0.5-2 parts of phenyl silicone oil, 20-30 parts of fumed silica, 5-15 parts of silicon carbide, 1-3 parts of hexamethyldisilazane, 1-3 parts of methyltrimethoxysilane, 5-10 parts of terminal hydrogen-containing silicone oil, 3-6 parts of side hydrogen-containing silicone oil, 0.1-0.5 parts of platinum catalyst, 0.005-0.1 parts of acetylene cyclohexanol and 0.5-3 parts of cerium isozincate; S2, put the vinyl-terminated silicone oil, polyvinyl silicone oil, vinyl silicone resin, hexamethyldisilazane and methyltrimethoxysilane into a vacuum kneader according to the proportion, and stir and knead for 20-30 minutes; S3, add fumed silica and silicon carbide into the kneader in 4-6 times according to the ratio, after adding, turn on the cooling water, and cold refine for 2-4 hours; S4. Turn on the vacuum pump, adjust the vacuum degree in the kneader to -0.1MPa, and continue to stir the material under vacuum conditions of 160℃-180℃ for 2-4h; S5. Stop vacuuming, open the vent valve, turn off the steam, turn on the cooling water, cool the material, and discharge the material after the material cools to below 50°C to obtain a wear-resistant liquid silicone base material; S6, transfer the wear-resistant liquid silicone base material into a special material tank of a vacuum high-speed mixer for standby use, and proceed to the next step of preparation; Phenyl silicone oil, terminal hydrogen silicone oil, side hydrogen silicone oil, acetylene cyclohexanol and cerium isozincate are added to the wear-resistant liquid silicone base material, and the mixture is vacuum stirred for 1-2 hours and then filtered and packaged with a 100-200 mesh filter to complete the preparation of the wear-resistant liquid silicone component A; S7, wear-resistant liquid silica gel B component, 5000ppm platinum catalyst; S8. Mix and stir the A and B component materials in a ratio of 100:0.3, pour the mixture into a mold for making a test piece, and then process it on a flat vulcanizer with a pressure of 13MPa, a temperature of 150°C and a curing time of 10min. After curing, a silicone test piece with good wear resistance can be obtained, and various physical properties can be tested.
5. The method for preparing high temperature resistant, high strength and wear resistant liquid silicone according to claim 4, characterized in that: In step S2, end-vinyl silicone oil, polyvinyl silicone oil, vinyl silicone resin, hexamethyldisilazane and methyltrimethoxysilane are put into the vacuum kneader at once, and stirring is started. During the stirring process, the preparation personnel closely observe the vacuum kneader and wait for the stirring and kneading to be completed.
6. The method for preparing high temperature resistant, high strength and wear resistant liquid silica gel according to claim 4, characterized in that: In step S3, after the stirring and kneading is completed, the fumed silica and silicon carbide are added in succession according to the ratio. During each addition, stirring is performed. After the addition is completed, the feed port of the kneader is closed and cold refining operation is performed.
7. The method for preparing high temperature resistant, high strength and wear resistant liquid silica gel according to claim 4, characterized in that: After the preliminary mixing and kneading is completed in step S4, the air and other non-condensable gases in the kneader are extracted by a vacuum pump, and the temperature is adjusted so that the internal structure of the material changes under the dual effects of high temperature and vacuum.
8. The method for preparing high temperature resistant, high strength and wear resistant liquid silica gel according to claim 4, characterized in that: In step S5, when the predetermined stirring time and heat treatment effect are achieved, the equipment is turned off, the vacuum degree in the kneader is slowly released to a normal pressure state, and the heat of the material and the inside of the equipment is taken away by cooling water.
9. The method for preparing high temperature resistant, high strength and wear resistant liquid silica gel according to claim 4, characterized in that: In step S8, an electronic scale is used to proportion the materials.
10. The method for preparing high temperature resistant, high strength and wear resistant liquid silica gel according to claim 4, characterized in that: In step S6, the uniformly stirred material is slowly poured into the filter press device, and pressure is applied to allow the material to pass through the filter screen to achieve solid-liquid separation.