Polymer SBS (Styrene Butadiene Styrene) modified asphalt compatilizer optimally prepared based on simplex gravity center design method

Optimized preparation of polymer SBS modified asphalt compatible agents through simplex center of gravity design method, using Jingmen extracted oil and rubber oil and other raw materials, solving the problems of high cost and poor performance of existing compatible agents, and achieving low temperature performance and resistance The improvement of aging performance simplifies the preparation process and reduces road construction costs.

CN119081424APending Publication Date: 2024-12-06LANZHOU JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411179957.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing SBS modified asphalt compatible agents have high cost, complex processes and poor performance, making it difficult to meet the needs of asphalt low-temperature performance and anti-aging performance.

Method used

The polymer SBS modified asphalt compatible agent optimized for preparation based on the simplex center of gravity design method is used. Jingmen extracted oil, rubber oil and plasticizer are used as raw materials. Jingmen extracted oil is waste engine oil, and the plasticizer is phthalic acid di- A mixture of butyl ester and din-butyl sebacate is prepared by heating and stirring, and a tackifier and a stabilizer are added to the asphalt to form a stable network structure.

Benefits of technology

It significantly reduces road construction costs, improves the compatibility, low temperature and anti-aging properties of SBS modified asphalt, simplifies the preparation process, and improves the accuracy and scientificity of the selection of compatible agent formulas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081424A_ABST
    Figure CN119081424A_ABST
Patent Text Reader

Abstract

The invention discloses a polymer SBS modified asphalt compatilizer optimally prepared based on a simplex gravity center design method, and relates to the field of road asphalt compatilizers. The SBS modified asphalt compatilizer is prepared from the following raw material components: chaste extract oil, rubber oil and a plasticizer, wherein the vitex extract oil is waste engine oil residual oil; the preferable weight ratio of m Jingmen extract oil to m rubber oil to m plasticizer is 64: 31: 5. The SBS modified asphalt compatilizer can effectively improve the compatibility problem of SBS modified asphalt, the SBS modified asphalt added with the compatilizer has good low-temperature performance and anti-aging performance, and meanwhile the SBS modified asphalt compatilizer has the advantages of being simple in preparation method and easy to control and is beneficial to application and popularization. According to the method, the optimal formula of the asphalt compatilizer is selected by adopting a simplex gravity center design, so that the accuracy and scientificity of formula selection of the asphalt compatilizer are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of road asphalt compatibilizers, in particular to a polymer SBS modified asphalt compatibilizer optimized and prepared based on a simplex centroid design method. Background Art

[0002] SBS modified asphalt is widely used in high-grade highway asphalt pavement due to its excellent performance. SBS modified asphalt is prepared by adding SBS modifier to base asphalt and undergoing a series of processes to improve the asphalt's ability to resist high and low temperatures and rutting. However, SBS modifier is suspended in asphalt in the form of adsorption and swelling. Long-term hot storage environment will cause the dispersed SBS particles to aggregate, destroying the phase distribution of SBS in asphalt and inducing the decay of asphalt rheological properties.

[0003] SBS modified asphalt can be expanded by adding admixtures to improve the compatibility between asphalt and polymer modifier SBS. Compatibilizers can effectively improve the expansion problem of SBS modifiers and asphalt systems, ensure that SBS is evenly dispersed in asphalt, and keep the cross-linked network structure of SBS in asphalt stable. Its main components are light components, including aromatics and saturated components. Between SBS modifiers and matrix asphalt, the interaction and aggregation between SBS modifiers and aromatic hydrocarbons are key factors to ensure their compatibility. The interaction and aggregation between saturated components help promote their compatibility. Compatibilizers can enhance the mobility between polymer segments and form a stable network structure in asphalt. Therefore, compatibilizers are an effective means to improve the compatibility of SBS modified asphalt.

[0004] The addition of stabilizers is a common means of increasing the volume. The most common raw material of stabilizers is mainly sulfur. It can form a stable interfacial adsorption layer between the polymers between the modifiers and asphalt, reduce the surface tension, and effectively improve the compatibility between SBS and asphalt, but the volume-increasing effect is limited. Compatibilizers can effectively improve the volume-increasing problem of SBS modifiers and asphalt systems, ensure that SBS is evenly dispersed in asphalt, and keep the cross-linked network structure of SBS in asphalt stable. Its main components are light components, including aromatics and saturated components. Between SBS modifiers and base asphalt, the interaction and aggregation between SBS modifiers and aromatic hydrocarbons are the key factors to ensure their compatibility. The interaction and aggregation between saturated components help promote their compatibility. Compatibilizers can enhance the mobility between polymer segments and form a stable network structure in asphalt. Therefore, compatibilizers are one of the effective means to improve the compatibility of SBS modified asphalt.

[0005] At present, the compatibilizers for modified asphalt are mainly oils with high saturated and aromatic contents. The addition of compatibilizers can significantly improve the compatibility between SBS and asphalt. But at the same time, the existing compatibilizers on the market can hardly meet the requirements of asphalt's low-temperature performance and anti-aging performance while increasing the volume of SBS modified asphalt. The use of compatibilizers is formulated based on experience, and high aromatic content is pursued blindly. While aromatic oil significantly improves the compatibility of modified asphalt, it has a negative impact on the road performance of asphalt. Simply using aromatic oil as a compatibilizer is difficult to meet the modification needs of modified asphalt. In order to solve the problems existing in the compatibilizer market, it is necessary to fully understand the effects of different types of compatibilizers on the performance of SBS modified asphalt, explore the laws of the effects of compatibilizers on asphalt performance, and develop compatibilizers that meet market demand. Summary of the invention

[0006] The purpose of the present invention is to provide a polymer SBS modified asphalt compatibilizer optimized and formulated based on the simplex centroid design method, so as to solve the problems of high cost, complex process and poor performance of the compatibilizer at this stage.

[0007] To achieve the above object, the present invention provides the following solutions:

[0008] One of the purposes of the present invention is to provide an SBS modified asphalt compatibilizer, the raw material components of which are as follows: Jingmen extracted oil, rubber oil and plasticizer; the Jingmen extracted oil is waste engine oil residue.

[0009] Furthermore, the plasticizer is a mixture of dibutyl phthalate (DBP) and di-n-butyl sebacate (DBS) in a mass ratio of 1:1.

[0010] Furthermore, the weight ratio of the Jingmen extracted oil, rubber oil, and plasticizer is: m 荆门抽出油 :m 橡胶油 :m 增塑剂 =64:31:5.

[0011] The second object of the present invention is to provide a method for preparing the above-mentioned SBS modified asphalt compatibilizer, comprising the following steps:

[0012] The Jingmen extracted oil and rubber oil are heated, and then the plasticizer is added, mixed, and stirred to obtain the SBS modified asphalt compatibilizer.

[0013] The third object of the present invention is to provide the use of the above-mentioned SBS modified asphalt compatibilizer in improving the compatibility of SBS modified asphalt.

[0014] Furthermore, the added amount of the SBS modified asphalt compatibilizer is 4% of the mass of the asphalt.

[0015] Furthermore, the application includes the following steps: heating the asphalt to a fluid state, adding the SBS modified asphalt compatibilizer and stirring to dissolve, then adding the SBS modifier and shearing, then adding a viscosity enhancer and a stabilizer and stirring to obtain SBS modified asphalt.

[0016] More preferably, the shearing time is 30 minutes, and the stirring time is 2.5 hours.

[0017] Furthermore, the added amount of the tackifier is 1% of the mass of the asphalt, and the added amount of the stabilizer is 0.3% of the mass of the asphalt; the tackifier is coumarone resin, and the stabilizer is a sulfur-based stabilizer.

[0018] The present invention adopts the oil extracted from Jingmen because it is low in cost and rich in saturated and aromatic components required for asphalt. After being added to SBS modified asphalt, it can supplement the light oil in the asphalt and make the SBS modifier fully swell.

[0019] When preparing polymer modified asphalt, good compatibility is the prerequisite for the preparation of modified asphalt and a necessary condition to ensure the excellent performance of the finished modified asphalt. The base asphalt has a low content of light components such as saturated components and aromatic components. By adding a compatibilizer to supplement the light components of SBS modified asphalt, SBS is fully swollen and more evenly distributed in the asphalt. This is also the main method for increasing the volume of the SBS modified asphalt system. After ensuring the volume-increasing effect of the addition of the compatibilizer on the asphalt system, it is also necessary to understand the effect of the addition of the compatibilizer on the performance of the asphalt to ensure the improvement of the performance of SBS modified asphalt in actual road applications.

[0020] In view of the influence of light components on the high-temperature properties of asphalt, it was found that the addition of compatibilizers will increase temperature sensitivity. Compatibilizers will cause changes in the viscoelastic ratio in SBS modified asphalt, gradually transforming from elastic to viscous components. This greatly reduces the deformation resistance of modified asphalt under high temperature conditions, indicating that compatibilizers are more sensitive to high-temperature performance. At the same time, the addition of compatibilizers can reduce the drainage resistance of asphalt, making asphalt easier to flow and deform. This property can effectively improve the low-temperature performance of asphalt. Its addition can reduce the maximum yield load of modified asphalt, increase the maximum tensile length before asphalt cracking, and effectively improve the low-temperature performance of asphalt.

[0021] The fourth object of the present invention is to provide a method for optimizing the formulation of the above-mentioned SBS asphalt compatibilizer based on simplex centroid design, comprising the following steps:

[0022] (1) Design the level corresponding to the raw material of the SBS asphalt compatibilizer and select an appropriate simplex centroid test scheme according to the number of factors and the component dosage range;

[0023] (2) preparing the SBS asphalt compatibilizer according to the design scheme, preparing SBS modified asphalt, and testing the basic indicators of the SBS modified asphalt;

[0024] (3) Using the simplex centroid design method theory, a structural model for the SBS asphalt compatibilizer formulation design is constructed, relevant parameters of the data set are calculated, and the contribution weight of the factor group to the target layer is obtained after a one-time test;

[0025] (4) According to Design-Expert 12.0 software, for the surrounding range value of the simplex centroid design result, the rubber oil, Jingmen extracted oil and plasticizer are used as independent variables, and the asphalt index is used as the response value y. Through experiments and computer models, the matrix method is used to solve the optimal parameter combination of the raw material dosage of the compatibilizer, and the basic performance indicators of asphalt are predicted through the prediction model.

[0026] Furthermore, the asphalt indicators include penetration, ductility and softening point.

[0027] The SBS modified asphalt compatibilizer of the present invention can effectively improve the compatibility problem of SBS modified asphalt. The SBS modified asphalt added with the compatibilizer of the present invention has good low temperature performance and anti-aging performance. At the same time, the present invention has the advantages of simple preparation method and easy control, which is conducive to popularization and application.

[0028] The present invention adopts a simplex centroid design to select the optimal formula of the asphalt compatibilizer, thereby improving the accuracy and scientificity of the selection of the asphalt compatibilizer formula.

[0029] The present invention discloses the following technical effects:

[0030] 1. The raw materials used for the compatibilizer prepared by the present invention are widely available and low in cost. It not only provides a new way for the environmental protection department to treat waste oil, but also, compared with ordinary compatibilizers on the market, uses low-priced wastes such as waste engine oil to significantly reduce the cost of road construction. When the SBS modified asphalt of the present invention is used, its ductility, residual ductility and separation softening point difference are restored to or even exceed those of the SBS modified asphalt without the addition of the compatibilizer.

[0031] 2. The present invention adopts the simplex centroid design method to select the optimal formula of asphalt compatibilizer, which not only reduces the number of tests and improves the test efficiency, but also avoids the defects of relying on subjective analysis when considering multiple indicators comprehensively, and improves the accuracy and scientificity of the selection of asphalt compatibilizer formula.

[0032] 3. The compatibilizer formula of the present invention is simple to operate, highly practical, and has accurate calculation results, which provides a basis for the efficient use of environmentally friendly compatibilizers. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0034] Figure 1 The ductility of asphalt with different formulations of compatibilizers added;

[0035] Figure 2 (a) is the asphalt ductility response distribution, (b) is the asphalt ductility response prediction distribution diagram;

[0036] Figure 3 The residual ductility of asphalt with different formulations of compatibilizers added;

[0037] Figure 4 (a) is the asphalt residual ductility response distribution, (b) is the asphalt residual ductility response prediction distribution diagram;

[0038] Figure 5 The residual ductility of asphalt with different formulations of compatibilizers added;

[0039] Figure 6 (a) is the asphalt segregation softening point difference response distribution, (b) is the asphalt segregation softening point difference response prediction distribution diagram;

[0040] Figure 7 The difference in the softening point of asphalt separation with different compatibilizers added;

[0041] Figure 8 (a) is the asphalt segregation softening point difference response distribution, (b) is the asphalt segregation softening point difference response prediction distribution diagram;

[0042] Fig. 9 Among them, (a) is the ductility prediction result, (b) is the softening point prediction result, (c) is the residual ductility prediction result, (d) is the segregation softening point difference prediction result, (e) is the rubber oil dosage, (f) is the Jingmen extracted oil dosage, and (g) is the plasticizer dosage. DETAILED DESCRIPTION

[0043] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0044] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0045] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0046] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0047] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0048] The present invention utilizes simplex centroid design to prepare an environmentally friendly road asphalt compatibilizer, comprising the following steps:

[0049] (1) Prepare SBS modified asphalt, and conduct indoor tests to select and study the main raw materials in the compatibilizer, determine the quantity of the main raw materials of the compatibilizer and the preliminary dosage range, and carry out detailed formula design;

[0050] (2) Based on the simplex centroid design, polymer SBS modified asphalt compatibilizers with different ratios were obtained. The effects of rubber oil, Jingmen extracted oil and plasticizer on the low-temperature performance of SBS modified asphalt were analyzed, and the synergistic effect of each component of the compatibilizer on asphalt was explored.

[0051] (3) Multi-factor simulation test: Design-Expert 12.0 software was used to target the range of values ​​around the simplex centroid design results. Rubber oil, Jingmen extracted oil, and plasticizer were used as independent variables, and asphalt ductility, residual ductility, and separation softening point difference were used as response values ​​y. Through repeated experiments and computer models, the matrix method was used to solve the optimal parameter combination of the raw material dosage of the compatibilizer, and the basic performance indicators of asphalt were predicted through the prediction model.

[0052] (4) Based on the simulation results of optimizing the compatibilizer formula parameters, the compatibilizer effect was experimentally verified, the model reliability was analyzed, and the optimal formula of the polymer SBS modified asphalt compatibilizer was obtained.

[0053] In the step (3), simulation models of asphalt ductility, residual ductility and separation softening point difference are established respectively, and the regression equations are ductility:

[0054] Y=58.37A+80.66B-6724.07C-17.05AB+7557.16AC+6134.26BC;

[0055] Softening point:

[0056] Y=51.41A+106.06B-8.402e 5 C-22.34AB+8.851e 5 AC+8.605e 5 BC-2.393e 5 A 2 BC-1.164e 5 AB 2 C+4.480e 6 ABC 2 ;

[0057] Residual ductility:

[0058] Y = 54.33A + 16.65B - 19.24C;

[0059] Segregation Softening Spread:

[0060] Y=2.15A-3.88B+1087.35C+14.09AB-1165.73AC-928.75BC-354.02ABC.

[0061] The weight percentages of the compatibilizer raw materials finally determined in step (4) are: 64% of rubber oil, 31% of Jingmen extracted oil, and 5% of plasticizer.

[0062] The error rates of the simulation results and the test results in step (4) are verified as follows: ductility 6.5%; residual ductility 1.9%; segregation softening point difference 1.4%, and the actual significant factor error rate is less than 7%.

[0063] The specific steps are as follows:

[0064] (1) Rubber oil and Jingmen extracted oil were swollen in a constant temperature oven at 100° C. for 30 h, and then a plasticizer (a mixture of DBP and DBS in a mass ratio of 1:1) and a tackifier (coumarone resin) were added and stirred for 10 minutes to obtain a mixture.

[0065] Rubber oil: Naphthenic oil can help SBS swell better in asphalt and improve the low temperature performance of modified asphalt. Naphthenic oil is also beneficial to the anti-aging performance of SBS modified asphalt. Studies have found that naphthenic oil can improve the compatibility of SBS modified asphalt, while improving low temperature performance and high temperature viscosity.

[0066] Jingmen extracted oil: With the depletion of oil resources, the cost of compatibilizers is getting higher and higher. The development of environmentally friendly compatibilizers has become a top priority. Waste oil has low cost and is rich in aromatic components required for asphalt. After being mixed with asphalt, it can supplement the light oil in asphalt, making the polymer SBS have good dispersibility and good compatibility with asphalt.

[0067] Plasticizer: Through research, it is found that plasticizer can significantly reduce the stiffness modulus of SBS modified asphalt and increase the creep rate. The improvement effect increases with the increase of plasticizer dosage. The addition of plasticizer makes the aging durability of SBS modified asphalt better than that of base asphalt, which is beneficial to improve the anti-aging performance of the road surface, slow down the aging of asphalt caused by the mixing and paving of asphalt mixture construction, and can slow down the low-temperature cracking.

[0068] Thickener: Through research, it is found that the thickener has good compatibility with polymer modifiers and is a solvent-based softener. It helps to disperse the modifier and can improve the asphalt process performance and enhance the physical and mechanical properties and aging resistance of asphalt.

[0069] (2) Preparation of SBS modified asphalt: First, the base asphalt was heated to about 160°C and the mixture of step (1) was added. Then, the sample preparation temperature was maintained at about 170°C and the SBS modifier was added batch by batch. The base asphalt and SBS modifier mixture was sheared at a speed of 5000 r / min for 30 min using a high-speed shearing machine. While the sample preparation temperature was maintained at about 170°C, a sulfur stabilizer was added to the modified asphalt, and the mixture was stirred at a speed of 1000 rpm / min for 2 h 30 min using a stirrer.

[0070] (3) Experimental design

[0071] From the asphalt compatibility mechanism, we can know that the compatibility technology is mainly to supplement the light oil in the asphalt, reduce the relative content of asphaltene, and make the SBS modifier absorb the light component and fully swell. At the same time, the low temperature performance and anti-aging property of the asphalt should be considered.

[0072] (4) Based on the simplex centroid design, the compatibilizer dosage of polymer SBS modified asphalt with different ratios is obtained. The specific steps are as follows:

[0073] Step 1: Design the level corresponding to the raw material of the compatibilizer, and select the appropriate simplex centroid test scheme according to the number of factors and levels. To ensure the effectiveness of the optimization results, the value targets of Jingmen extracted oil, rubber oil, and plasticizer are set to "within the bounds". According to the qualified range of the basic indicators of 90# matrix asphalt specified in the specification, the three response value boundary ranges of ductility, residual ductility, and segregation softening point difference are set respectively, and the design parameters are shown in Table 1.

[0074] Table 1 The dosage range of each component of compatibilizer

[0075]

[0076]

[0077] A simplex centroid design consisting of three components was conducted for Jingmen extracted oil, rubber oil and plasticizer. The experimental scheme was designed using the mixture simplex centroid method in the Design-Expert software. The design scheme is shown in Table 2. The total number of test points is 10, and the values ​​are rounded to two decimal places.

[0078] Table 2 Compatibilizer simplex centroid test scheme

[0079]

[0080] Step 2: prepare a compatibilizer according to the simplex centroid design scheme and test the basic indicators of SBS modified asphalt.

[0081] The low-temperature performance of asphalt can be reflected by ductility, the anti-aging performance can be reflected by the residual ductility, and the segregation softening point difference can reflect the compatibility of asphalt. By analyzing the improvement of asphalt performance by compatibilizers under various composition ratios, Design-Expert is used to analyze the contribution of each component of the compatibilizer to the performance, and a prediction model is constructed, based on which the compatibilizer composition design is optimized. During the experiment, the penetration, ductility, softening point, penetration reduction, ductility reduction, and segregation softening point difference indicators were determined, and the ductility, residual ductility, and segregation softening point difference indicators were analyzed in detail. The composition design scheme was optimized and verified. For the 6 indicators measured, it is required to meet the requirements of the specification JTG f40-2004 "Technical Specifications for Highway Asphalt Pavement Construction" IB and DB15 / T 2281-2021 "Technical Specifications for Cold Regeneration of Emulsified Asphalt in Cold Regions Highway Asphalt Pavement". The test results are shown in Table 3.

[0082] Table 3 Basic data of asphalt with low temperature compatibilizer added at different material mix ratios

[0083]

[0084]

[0085] Step 3, multi-factor simulation test: The present invention uses Design-Expert 12.0 software to select the peripheral range values ​​of the results for different indicators, designs a multi-factor orthogonal rotation combination test, takes Jingmen extracted oil, rubber oil, and plasticizer as independent variables, and takes asphalt ductility, residual ductility, and separation softening point difference as response value y. Through repeated experiments and computer models, the matrix method is used to solve the optimal parameter combination of each raw material dosage of the compatibilizer, and the basic performance indicators of asphalt are predicted by computer.

[0086] At a 5% compatibilizer dosage, the ductility of the 10 groups of asphalts is greater than the 40cm required by the specification, ensuring the low-temperature performance of the asphalt. Among them, the maximum ductility value of the A8 sample can reach 79.6, while the minimum ductility value of the A3 sample is only 43.2. The ductility of the A1 sample composed only of Jingmen extracted oil and the A10 sample composed only of rubber oil in the compatibilizer composition is 61.20cm and 43.60cm. The ductility of these two groups of asphalt samples is lower than the A8 point, so it can be considered that there is a synergistic effect between Jingmen extracted oil and rubber oil that promotes the growth of the asphalt ductility index. At the same time, it is necessary to refine the research on the ratio of the compatibilizer. Under the ratios of A4, A5, and A8 groups, the ductility of the asphalt samples is greater than that of the A1 group asphalt.

[0087] Table 4 Ductility fitting data

[0088]

[0089] Table 5 Delay coding factor coefficients

[0090]

[0091] From the results of the ductility fitting analysis in Table 4, we can see that the average value of the ductility model is 61.99, and the model R 2 The value is 0.4837, and the adjusted model determines R 2 The value of the regression equation is 0.161, and the prediction model accuracy is 4.3147. The above analysis shows that the regression equation can predict the test results with sufficient accuracy. There is a certain deviation between the measured value of asphalt ductility and the predicted straight line. The fitting formula is shown in Formula 1. According to the fitting formula, it can be found that the various components of the compatibilizer have a synergistic effect on the ductility of asphalt.

[0092] Elongation = 58.37A + 80.66B - 6724.07C - 17.05AB + 7557.16AC + 6134.26BC (1)

[0093] Among them, A represents the percentage of rubber oil in the mass of compatibilizer, B represents the percentage of Jingmen extracted oil in the mass of compatibilizer, and C represents the percentage of plasticizer in the mass of compatibilizer.

[0094] The softening point characterizes the temperature sensitivity of asphalt. At a compatibilizer dosage of 5%, the ductility of the 10 groups of asphalts was greater than the 50°C required by the specification, ensuring the high temperature performance of the asphalt. Among them, the softening point value of the A4 sample can reach a maximum of 80.05, while the softening point value of the A9 sample is only 52.20. The softening points of the A1 sample composed only of Jingmen extracted oil and the A10 sample composed only of rubber oil in the compatibilizer composition are 72.00cm and 65.10cm. The softening points of these two groups of asphalt samples are lower than the A4 point, so it can be considered that the synergistic effect between Jingmen extracted oil and rubber oil promotes the growth of the asphalt softening point index. At the same time, the ratio of the compatibilizer needs to be refined.

[0095] Table 6 Softening point fitting data

[0096]

[0097] Table 7 Softening point coding factor coefficient

[0098]

[0099] From the results of the ductility fitting analysis in Table 6, we can see that the average value of the ductility model is 71.76, and the model R 2 The value is 0.6193. Through the above analysis, it can be seen that the regression equation can predict the test results with sufficient accuracy. There is a certain deviation between the measured value of asphalt ductility and the predicted straight line. The fitting formula is shown in Formula 2. According to the fitting formula, it can be found that the various components of the compatibilizer have a synergistic effect on the ductility of asphalt.

[0100] Softening point = 51.41A + 106.06B - 8.402*10 5 C-22.34AB+8.851*10 5 AC+8.605*10 5 BC-2.393*10 5 A 2 BC-1.164*10 5 AB 2 C+4.48*10 6 ABC 2 (2)

[0101] Residual ductility refers to the measurement of asphalt ductility after the base asphalt undergoes RTFOT short-term aging. This data can effectively reflect the low-temperature anti-aging performance of asphalt. Test results of residual ductility of A1-A10 asphalt at 5°C. The experimental results of residual ductility at 5°C vary greatly, ranging from 28.1 to 55.5; by comparison, the results of the reduction in ductility after asphalt undergoes RTFOT short-term aging can be analyzed. The maximum residual ductility value of the A1 sample can reach 55.5, and the ductility decreases the least, only 9.31%. The ductility of the A8 sample decreases the most, by 54.77%, and this group of asphalt has the worst anti-aging performance. The residual ductility shows an overall downward trend as the rubber oil content decreases. It can be inferred that rubber oil can improve the low-temperature performance of asphalt after aging.

[0102] Table 8 Residual ductility fitting data

[0103]

[0104] Table 9 Residual ductility coding factor coefficient

[0105]

[0106] From the residual ductility fitting analysis results in Table 8, it can be seen that the average value of the residual ductility model is 35.04, and the model R 2 The value is 0.5044, and the adjusted model determines R 2 The value of the regression equation is 0.4142, and the prediction model accuracy is 6.4181. The above analysis shows that the regression equation can predict the test results with sufficient accuracy. There is a certain deviation between the measured value of the residual ductility of asphalt and the predicted straight line. The fitting formula is shown in Formula 3. According to the fitting formula, it can be found that the components of the compatibilizer are linearly related to the residual ductility of asphalt.

[0107] Residual ductility = 54.33A + 16.65B - 19.24C (3)

[0108] Segregation softening point difference refers to the difference between the softening points of the asphalt at the top and bottom of the storage tube after the base asphalt has been aged for 48 hours. This data can effectively reflect the compatibility of SBS modified asphalt. Test results of the segregation softening point difference of A1-A10 asphalt samples. Among them, the asphalt segregation softening point difference of A3 and A6 samples exceeds the 2.5℃ required by the specification, which does not meet the asphalt production needs. The compatibilizer of the A1 asphalt sample is only composed of Jingmen extracted oil, and the segregation softening point difference of the specimen is the smallest, which is 0.7℃. In the A2-A9 system where Jingmen extracted oil and rubber oil are mixed, after removing the A3 abnormal point, it is found that with the increase of the rubber oil content, the segregation softening point difference of the asphalt sample basically shows a trend of first rising and then falling. The segregation softening point difference of asphalt sample A9 is the lowest, which is 1.1℃.

[0109] Table 10 Segregation softening point difference fitting data

[0110]

[0111] Table 11 Segregation Softening Spread Coding Factor Coefficients

[0112]

[0113]

[0114] From the fitting analysis results of the segregation softening point difference in Table 10, it can be seen that the average value of the segregation softening point difference model is 9.56, and the model R 2 The value is 0.9980, and the adjusted model determines R 2 The above analysis shows that the regression equation can predict the test results with sufficient accuracy. There is a certain deviation between the measured value of the asphalt segregation softening point difference and the predicted straight line. The fitting formula is shown in Formula 4. According to the fitting formula, it can be found that the components of the compatibilizer have a synergistic effect on the asphalt segregation softening point difference.

[0115] Segregation softening point difference = 2.15A-3.88B+1087.35C+14.09.AB-1165.73AC-928.75BC-354.02ABC (4)

[0116] In order to design a compatibilizer that takes into account both low temperature resistance and anti-aging performance, the present invention uses 5°C ductility as the main indicator to evaluate the low temperature effect of the compatibilizer on SBS modified asphalt, and 5°C residual ductility as a secondary indicator to evaluate the anti-aging effect of the compatibilizer on SBS modified asphalt. In addition, to ensure the effective role of the compatibilizer in SBS modified asphalt, the segregation softening point is used as a supplementary reference indicator. According to existing research results and specifications, the 5°C ductility of SBS modified asphalt after adding the compatibilizer should not be less than 40cm, and the segregation softening point difference should not be higher than 2.5°C. On this basis, the greater the 5°C residual ductility, the better the anti-aging performance of the asphalt. Based on this, the optimization of the compatibilizer composition design ratio is carried out.

[0117] Parameter optimization and comparative test: For the regression model of ductility, residual ductility, and segregation softening point difference, the Optimization function in DesignExpert 12.0 is used to solve the regression model and obtain the optimal solution for model optimization design as shown in Table 12 and Fig. 9 shown.

[0118] Table 12 Design-Expert optimization solution for compatibilizer ratio and asphalt performance prediction

[0119]

[0120] According to the planning solution results of the simplex centroid design and the optimization of the formula, the relevant data are shown in Table 12. The predicted result of the ductility obtained in the model is 47.51cm, the predicted result of the residual ductility is 39.03cm, and the predicted result of the softening point is 54.81℃.

[0121] Table 13 Compatibilizer optimization formula verification and relative error calculation

[0122]

[0123] According to the results in Table 13, the compatibilizer was configured with the above ratio and added to SBS modified asphalt at a dosage of 4% of the asphalt mass. The ductility, residual ductility and segregation softening point difference of the asphalt were measured. By calculating the relative error between the predicted value and the measured value, the results show that the prediction of residual ductility and segregation softening point difference is relatively accurate, and the relative error can be controlled within 5%. However, the prediction deviation of ductility is large, and the absolute value of the relative error reaches 6.5%. This is consistent with the previous research conclusions, that is, the response surface fitting accuracy of residual ductility and softening point is high, while the fitting of asphalt ductility is relatively poor.

[0124] The prediction results of the optimized formula of Design-Expert are reasonable and meet the expected use requirements. Therefore, the present invention adopts the above-mentioned SBS modified asphalt compatibilizer ratio to carry out subsequent related tests, that is, the blending ratio of rubber oil: Jingmen extracted oil: plasticizer is about 64:31:5.

[0125] Performance verification based on the implementation plan asphalt compatibilizer:

[0126] After determining the compatibilizer formula, its physical indicators were tested, and the specific contents are shown in Table 14. By analyzing the chemical composition of the compatibilizer, it can be found that the main chemical composition of the compatibilizer is saturated fraction, which accounts for 61.31% of the total volume. The aromatic fraction content accounts for 28.43% of the total volume, second only to the saturated fraction. The light component content accounts for 89.74% of the total compatibilizer, and the asphaltene and colloid in the heavy component only account for 0.73% and 9.53% of the total volume of the compatibilizer. Therefore, the addition of the compatibilizer can effectively increase the light component content of SBS modified asphalt, soften the asphalt, and affect the asphalt performance.

[0127] Table 14 Technical indicators of compatibilizer

[0128]

[0129] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A SBS modified asphalt compatibilizer, characterized in that: The raw material components are as follows: Jingmen extracted oil, rubber oil and plasticizer; the Jingmen extracted oil is waste engine oil residue.

2. The SBS modified asphalt compatibilizer according to claim 1, characterized in that: The plasticizer is a mixture of dibutyl phthalate and di-n-butyl sebacate in a mass ratio of 1:

1.

3. The SBS modified asphalt compatibilizer according to claim 1, characterized in that: The weight ratio of Jingmen extracted oil, rubber oil and plasticizer is: 荆门抽出油 :m 橡胶油 :m 增塑剂 =64:31:

5.

4. The method for preparing the SBS modified asphalt compatibilizer according to any one of claims 1 to 3, characterized in that: The following steps are involved: The Jingmen extracted oil and rubber oil are heated, and then the plasticizer is added, mixed, and stirred to obtain the SBS modified asphalt compatibilizer.

5. Use of the SBS modified asphalt compatibilizer as described in any one of claims 1 to 3 in improving the compatibility of SBS modified asphalt.

6. The use according to claim 5, characterized in that: The added amount of the SBS modified asphalt compatibilizer is 4% of the mass of the asphalt.

7. The use according to claim 5, characterized in that: The method comprises the following steps: heating the asphalt to a fluid state, adding the SBS modified asphalt compatibilizer to stir and dissolve, then adding the SBS modifier to shear, then adding a tackifier and a stabilizer, stirring to obtain the SBS modified asphalt.

8. The use according to claim 7, characterized in that: The added amount of the tackifier is 1% of the mass of the asphalt, and the added amount of the stabilizer is 0.3% of the mass of the asphalt; the tackifier is coumarone resin, and the stabilizer is a sulfur stabilizer.

9. A method for optimizing the formulation of the SBS asphalt compatibilizer according to any one of claims 1 to 3 based on simplex centroid design, characterized in that: The following steps are involved: (1) Design the level corresponding to the raw material of the SBS asphalt compatibilizer and select an appropriate simplex centroid test scheme according to the number of factors and the component dosage range; (2) preparing the SBS asphalt compatibilizer according to the design scheme, preparing SBS modified asphalt, and testing the basic indicators of the SBS modified asphalt; (3) Using the simplex centroid design method theory, a structural model for the SBS asphalt compatibilizer formulation design is constructed, relevant parameters of the data set are calculated, and the contribution weight of the factor group to the target layer is obtained after a one-time test; (4) According to Design-Expert 12.0 software, for the surrounding range value of the simplex centroid design result, the rubber oil, Jingmen extracted oil and plasticizer are used as independent variables, and the asphalt index is used as the response value y. Through experiments and computer models, the matrix method is used to solve the optimal parameter combination of the raw material dosage of the compatibilizer, and the basic performance indicators of asphalt are predicted through the prediction model.

10. The method according to claim 9, characterized in that The asphalt indicators include needle penetration, ductility and softening point.