Transparent insect-proof self-repairing fireproof coating for ancient buildings and preparation method thereof

By using hindered urea structure and hydrogen bonds in transparent fire-resistant coatings, self-healing and ultraviolet absorption are achieved, and the problem of difficult scratches and UV blocking in the prior art is solved, and the durability and protective performance of the coating is improved.

CN119081523AActive Publication Date: 2024-12-06SICHUAN FIRE RES INST OF MEM
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411294366.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-12-06
Estimated Expiration
2044-09-14

AI Technical Summary

Technical Problem

The existing transparent fire-resistant coating is difficult to prevent scratches and cannot completely block UV rays, causing rapid aging of wood, requiring additional UV absorbers to be added, affecting the coating film formation effect.

Method used

Using amino resins, isophorone diisocyanate, ethylene-ethylene acetate copolymer, polyvinyl alcohol, phosphonium phosphonate, guanidine phosphate, zirconium borate, pentaerythritol, phytic acid and film-forming additives, through hindered urea structure and hydrogen bonds Form a three-dimensional network structure to achieve self-healing and ultraviolet absorption.

Benefits of technology

Without adding ultraviolet absorbers, the coating can self-heal fine scratches, improve durability and insect resistance, while enhancing the absorption effect of ultraviolet rays and extending the protective performance of the coating.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a transparent insect-proof self-repairing fireproof coating for ancient buildings and a preparation method of the transparent insect-proof self-repairing fireproof coating, and relates to the technical field of wood building protection. The coating comprises amino resin, isophorone diisocyanate, an ethylene-ethylene acetic acid copolymer, polyvinyl alcohol, phosphorus nitrogen phosphonate, guanidine phosphate, zirconium borate, pentaerythritol, phytic acid and a film-forming additive. The isophorone diisocyanate is used as a curing agent of the amino resin; the isophorone diisocyanate is connected with the amino resin through a hindered urea structure; the hindered urea structure is used for self-repairing and forming a hydrogen bond with the phytic acid; according to the preparation method, the coating can be used for self-repairing tiny scratches, and the coating can absorb ultraviolet rays and reduce the wood aging speed under the condition that an ultraviolet light absorber is not additionally arranged. The purpose that the prepared coating can have hydrogen bonds for absorbing ultraviolet rays and can be used for self-repairing a hindered urea structure is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wooden building protection, in particular to a transparent insect-proof self-repairing ancient building fireproof coating and a preparation method thereof. Background Art

[0002] Many ancient wooden buildings in my country have inestimable historical and cultural values. However, the characteristics of their wooden structures make them fire-hazardous. Once a fire occurs, it is very easy to cause irreparable losses. Therefore, it is necessary to strengthen the fire protection of ancient buildings. Transparent fire-retardant coating is a type of decorative fire-retardant coating that can maintain the appearance of the substrate and meet the needs of fire protection.

[0003] The transparent fireproof coating is used to protect the surface of ancient buildings without changing the appearance and color of the ancient buildings. When it encounters fire, it can expand and form a uniform and dense honeycomb or sponge-like carbon foam layer, which has a good protective effect on combustible ancient buildings, so that the ancient buildings are not damaged by fire, so as to ensure the fire safety of these ancient buildings and prevent fire hazards before they happen. It plays an important role in the fire safety measures of ancient buildings. Therefore, the society has put forward very urgent requirements for transparent fireproof coatings. At present, there are only one or two varieties of transparent fireproof coatings that have been formally identified in China, which is far from meeting the needs of society. In addition, the transparent fireproof coating products on the market cannot meet the actual needs of the wooden structure of ancient buildings for insect resistance, moisture resistance, durability and weather resistance. Therefore, further research on insect-proof, durable and weather-resistant transparent fireproof coatings is necessary to enable more and better products to be launched and adapt to the development and needs of society. It is not only very necessary, but also has important significance for the protection of ancient buildings.

[0004] Transparent fireproof coating is a new type of fireproof technology developed in recent years. The product is mainly used for fire protection of high-grade wood decorative materials and ancient buildings that do not affect the appearance and color. The transparent fireproof coating is used as the exterior layer of high-grade wood decorative materials and ancient buildings. Its decorative effect is similar to other varnishes, and it can also play a role in fire protection. Transparent fireproof coating is generally based on artificially synthesized organic polymer resin. Sometimes the organic polymer resin is modified with special groups. The resin itself can carry a certain amount of flame retardant groups and foaming groups. A small amount of foaming agent, flame retardant, carbon source, etc. are appropriately added to form a fireproof system. In order to ensure the fireproof and other performance of the coating, a transparent topcoat is required in some occasions.

[0005] The UN-C30 water-based transparent fireproof coating developed by Beijing Youansheng Fireproof Technology Co., Ltd. is a fireproof coating composed of modified amino resin as base material, phosphoric acid and ammonium polyphosphate as dehydration catalysts, pentaerythritol as carbonizing agent, melamine and urea as foaming agents, and water as solvent. The L-1 transparent fireproof coating developed by Northeastern University is a water-soluble intumescent transparent fireproof coating. After the coating is dried, a waterproof film is formed, which solves the water resistance of the coating and does not require a topcoat. This is a completely different advantage from other transparent fireproof coatings. The boric acid ester fireproof coating synthesized by Chengde Petroleum College is obtained by replacing oligomer amino resin with high polymer amino resin, ammonium polyborate with ammonium borate, and dipentaerythritol with pentaerythritol. The fireproof effect of this coating is greatly enhanced, which can meet the fire protection needs of general materials and is also the direction of future research. The intumescent transparent fire-retardant coating developed by Henan Institute of Chemistry is made of isopropyl alcohol-modified melamine urea-formaldehyde resin as the base material and homemade chloroethyl phosphate as the flame retardant.

[0006] Chinese patent CN106634394B discloses a water-based transparent fire-retardant coating for ancient buildings and its preparation method, which improves the fire-retardant performance of the coating. The coating is transparent, can maintain the original appearance of the material, is not easy to crack, and has good weather resistance. The main component of the invention is dry powder type, which effectively prolongs the shelf life of the coating. Storage period: adding water-based wood stabilizer and phytic acid into fire-retardant coating can effectively protect the wood from rotting and deformation.

[0007] However, the existing technology has the problem of being difficult to prevent scratches, and in order to prevent the transparent coating from failing to completely block ultraviolet rays and causing rapid aging of the wood, it is necessary to add additional ultraviolet absorbers, which are one of the external fillers and have a certain influence on the film-forming effect of the coating. For the three-dimensional network structure formed by the curing of the resin, the more external fillers there are, the worse the density of the network structure will be, thereby reducing the film-forming effect of the coating. Summary of the invention

[0008] One of the purposes of the present invention is to provide a transparent insect-proof self-repairing ancient building fire-retardant coating, so that the coating can self-repair fine scratches, and without adding ultraviolet absorbers, it can absorb ultraviolet rays and reduce the aging rate of wood.

[0009] In order to achieve the above object, the present invention adopts the following technical means: A transparent insect-proof self-repairing ancient building fireproof coating, comprising amino resin, isophorone diisocyanate, ethylene-vinyl acetate copolymer, polyvinyl alcohol, phosphonitrile phosphate, guanidine phosphate, zirconium borate, pentaerythritol, phytic acid and film-forming additives; The isophorone diisocyanate is used as a curing agent for the amino resin; The isophorone diisocyanate and the amino resin are connected via a hindered urea structure; The hindered urea structure is used for self-repair and hydrogen bonding with the phytic acid.

[0010] The isocyanate groups at both ends of isophorone diisocyanate react with the amino groups in the amino resin, and isophorone diisocyanate is used as a connecting segment to form a three-dimensional network structure in the coating body. Under a specific preparation method, a hindered urea structure is formed between the amino groups of isophorone diisocyanate and the amino resin. When a fine scratch occurs on the coating surface, part of the chain segments of the coating are disconnected. Under the action of ultraviolet rays and the initiating factors in the coating, the hindered urea structure is constantly relinked. At the same time, under the action of the initiating factors, the free amino groups and isocyanate groups in the coating system are constantly combined to form a new hindered urea structure, thereby realizing self-repair of fine scratches on the coating surface under sunlight. Improve the durability and insect resistance of the coating.

[0011] The aforementioned triggering factor is the hydrogen bond formed between the hindered urea structure and phytic acid. When ultraviolet rays enter the coating, they are absorbed by the hydrogen bonds, which absorb energy and break, thereby releasing energy, which is used to generate the hindered urea structure. This not only repairs the fine scratches on the coating surface, but also the three-dimensional network structure in the coating becomes denser as the use time increases, and the protective performance of the coating becomes better and better as time goes by.

[0012] In addition, multiple hydrogen bonds can be formed between phytic acid and hindered urea structures, thereby greatly increasing the coating's absorption of ultraviolet rays.

[0013] Furthermore, the film-forming additives include a thickening and leveling agent, a wetting and dispersing agent, a film-forming aid PPH, a defoaming agent and a wood stabilizer MJB-TF.

[0014] Furthermore, the invention comprises, by weight, 30-40 parts of amino resin, 1-5 parts of isophorone diisocyanate, 1-5 parts of ethylene-vinyl acetate copolymer, 3-5 parts of polyvinyl alcohol, 5-10 parts of phosphonitrile phosphate, 5-10 parts of guanidine phosphate, 1-3 parts of zirconium borate, 5-10 parts of pentaerythritol, 3-6 parts of phytic acid, 0.5-1 parts of thickening and leveling agent, 0.5-1 parts of wetting and dispersing agent, 0.5-1 parts of film-forming aid PPH, 0.5-1 parts of defoaming agent and 0.5-1 parts of wood stabilizer MJB-TF.

[0015] The ethylene-vinyl acetate copolymer and polyvinyl alcohol used in the present invention can increase the flexibility of the paint film; in the entire coating system, there is no need to add an additional ultraviolet absorber, and the coating can be prepared normally to ensure the coating performance while absorbing ultraviolet rays. Phytic acid, as a substance that prevents wood from rotting and oxidation, is also necessary for the protection of wooden buildings.

[0016] Furthermore, another object of the present invention is to provide a method for preparing the aforementioned transparent insect-proof self-repairing ancient building fire-retardant coating, so as to achieve the purpose of enabling the prepared coating to have hydrogen bonds for absorbing ultraviolet rays and for self-repairing obstructed urea structures.

[0017] In order to achieve the above object, the present invention adopts the following technical means: A method for preparing the aforementioned transparent insect-proof self-repairing ancient building fire-retardant coating comprises: Initial mixing: adding amino resin, ethylene-vinyl acetate copolymer, polyvinyl alcohol, phosphonitrile phosphate, guanidine phosphate, zirconium borate, pentaerythritol and phytic acid into acetone solvent, stirring and mixing to obtain mixture A; Final mixing: adding a film-forming additive to the mixture A, adding triethanolamine to adjust the pH of the reaction step to alkaline, and then adding isophorone diisocyanate, stirring in a dark room environment, stirring evenly, and performing high-temperature curing in a dark room environment for 1 to 2 days to obtain the fire retardant coating.

[0018] Preferably, in the final mixing step, the pH is 8-9.

[0019] Furthermore, in the final mixing step, the curing temperature is 70-80°C.

[0020] Among them, pH value and temperature are more stringent reaction conditions. If the pH value is small and the temperature is lower than 70°C, a hindered urea structure cannot be formed between isophorone diisocyanate and the amino resin. The curing in this state is completely formed by the self-curing of the amino resin, and a three-dimensional network structure cannot be formed. The mechanical properties of the coating are poor, and a large number of hydrogen bonds cannot be formed inside it, and ultraviolet rays cannot be absorbed well. At the same time, the coating cannot self-repair after scratches.

[0021] When the pH value is greater than 9, although a three-dimensional network structure can be formed after curing and the mechanical properties of the coating are better, the purpose of self-repair cannot be achieved in practice. When the pH value is greater than 9, the hydrogen bonds formed in the system will be destroyed, resulting in the inability to effectively absorb ultraviolet rays under sunlight. Therefore, the aforementioned initiating factors cannot take effect and cannot promote the re-generation of the hindered urea structure.

[0022] Therefore, the method provided by the present invention is used to prepare the corresponding coating, which not only enables the coating to have the effects of self-repair and ultraviolet absorption, but also can be prepared in a dark room to avoid excessive cross-linking and rapid curing during the preparation process, causing large internal stress in the coating, and easy to fall off from the surface of the wooden building. DETAILED DESCRIPTION

[0023] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments.

[0024] Therefore, the following detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features of the embodiments may be combined with each other.

[0026] A transparent insect-proof self-repairing ancient building fireproof coating, comprising amino resin, isophorone diisocyanate, ethylene-vinyl acetate copolymer, polyvinyl alcohol, phosphonitrile phosphate, guanidine phosphate, zirconium borate, pentaerythritol, phytic acid and film-forming additives; The isophorone diisocyanate is used as a curing agent for the amino resin; The isophorone diisocyanate and the amino resin are connected via a hindered urea structure; The hindered urea structure is used for self-repair and hydrogen bonding with the phytic acid.

[0027] The isocyanate groups at both ends of isophorone diisocyanate react with the amino groups in the amino resin, and isophorone diisocyanate is used as a connecting segment to form a three-dimensional network structure in the coating body. Under a specific preparation method, a hindered urea structure is formed between the amino groups of isophorone diisocyanate and the amino resin. When a fine scratch occurs on the coating surface, part of the chain segments of the coating are disconnected. Under the action of ultraviolet rays and the initiating factors in the coating, the hindered urea structure is constantly relinked. At the same time, under the action of the initiating factors, the free amino groups and isocyanate groups in the coating system are constantly combined to form a new hindered urea structure, thereby realizing self-repair of fine scratches on the coating surface under sunlight. Improve the durability and insect resistance of the coating.

[0028] The aforementioned triggering factor is the hydrogen bond formed between the hindered urea structure and phytic acid. When ultraviolet rays enter the coating, they are absorbed by the hydrogen bonds, which absorb energy and break, thereby releasing energy, which is used to generate the hindered urea structure. This not only repairs the fine scratches on the coating surface, but also the three-dimensional network structure in the coating becomes denser as the use time increases, and the protective performance of the coating becomes better and better as time goes by.

[0029] In addition, multiple hydrogen bonds can be formed between phytic acid and hindered urea structures, thereby greatly increasing the coating's absorption of ultraviolet rays.

[0030] Furthermore, the film-forming additives include a thickening and leveling agent, a wetting and dispersing agent, a film-forming aid PPH, a defoaming agent and a wood stabilizer MJB-TF.

[0031] Furthermore, the invention comprises, by weight, 30-40 parts of amino resin, 1-5 parts of isophorone diisocyanate, 1-5 parts of ethylene-vinyl acetate copolymer, 3-5 parts of polyvinyl alcohol, 5-10 parts of phosphonitrile phosphate, 5-10 parts of guanidine phosphate, 1-3 parts of zirconium borate, 5-10 parts of pentaerythritol, 3-6 parts of phytic acid, 0.5-1 parts of thickening and leveling agent, 0.5-1 parts of wetting and dispersing agent, 0.5-1 parts of film-forming aid PPH, 0.5-1 parts of defoaming agent and 0.5-1 parts of wood stabilizer MJB-TF.

[0032] The ethylene-vinyl acetate copolymer and polyvinyl alcohol used in the present invention can increase the flexibility of the paint film; in the entire coating system, there is no need to add an additional ultraviolet absorber, and the coating can be prepared normally to ensure the coating performance while absorbing ultraviolet rays. Phytic acid, as a substance that prevents wood from rotting and oxidation, is also necessary for the protection of wooden buildings.

[0033] Furthermore, another object of the present invention is to provide a method for preparing the aforementioned transparent insect-proof self-repairing ancient building fire-retardant coating, so as to achieve the purpose of enabling the prepared coating to have hydrogen bonds for absorbing ultraviolet rays and for self-repairing obstructed urea structures.

[0034] In order to achieve the above object, the present invention adopts the following technical means: A method for preparing the aforementioned transparent insect-proof self-repairing ancient building fire-retardant coating comprises: Initial mixing: adding amino resin, ethylene-vinyl acetate copolymer, polyvinyl alcohol, phosphonitrile phosphate, guanidine phosphate, zirconium borate, pentaerythritol and phytic acid into acetone solvent, stirring and mixing to obtain mixture A; Final mixing: adding a film-forming additive to the mixture A, adding triethanolamine to adjust the pH of the reaction step to alkaline, and then adding isophorone diisocyanate, stirring in a dark room environment, stirring evenly, and performing high-temperature curing in a dark room environment for 1 to 2 days to obtain the fire retardant coating.

[0035] Preferably, in the final mixing step, the pH is 8-9.

[0036] Furthermore, in the final mixing step, the curing temperature is 70-80°C.

[0037] Among them, pH value and temperature are more stringent reaction conditions. If the pH value is less than 8 and the temperature is lower than 70°C, a hindered urea structure cannot be formed between isophorone diisocyanate and the amino resin. The curing in this state is completely formed by the self-curing of the amino resin, and a three-dimensional network structure cannot be formed. The mechanical properties of the coating are poor, and a large number of hydrogen bonds cannot be formed inside it, and ultraviolet rays cannot be absorbed well. At the same time, the coating cannot self-repair after scratches.

[0038] When the pH value is greater than 9, although a three-dimensional network structure can be formed after curing and the mechanical properties of the coating are better, the purpose of self-repair cannot be achieved in practice. When the pH value is greater than 9, the hydrogen bonds formed in the system will be destroyed, resulting in the inability to effectively absorb ultraviolet rays under sunlight. Therefore, the aforementioned initiating factors cannot take effect and cannot promote the re-generation of the hindered urea structure.

[0039] Therefore, the method provided by the present invention is used to prepare the corresponding coating, which not only enables the coating to have the effects of self-repair and ultraviolet absorption, but also can be prepared in a dark room to avoid excessive cross-linking and rapid curing during the preparation process, causing large internal stress in the coating, and easy to fall off from the surface of the wooden building.

[0040] Example 1 The coating is prepared by adopting the formula and preparation method of the present invention.

[0041] Example 2 The reaction pH in Example 1 was adjusted to less than 8.

[0042] Example 3 The reaction pH in Example 1 was adjusted to be greater than 9.

[0043] Example 4 The curing temperature in Example 1 was set to less than 70°C.

[0044] Example 5 The curing temperature in Example 1 was set to be greater than 80°C.

[0045] After comparing Examples 1 to 5, although the mechanical properties of the coatings in Examples 5 and 3 are improved, the problems they bring are that the coating curing time is too fast, the coating shrinks severely, the adhesion is greatly reduced, and the coating cannot self-repair, and the hydrogen bonds in the coating are greatly damaged.

[0046] In Example 2 and Example 4, although the coating can be cured, the mechanical properties of the coating are significantly reduced, and it is unable to self-repair and absorb a large amount of ultraviolet rays. This means that not only is there no hindered urea structure formed inside, but there are also no large amounts of hydrogen bonds to absorb ultraviolet rays. In this case, an external ultraviolet absorber is required to use the transparent coating to protect the wooden building.

[0047] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A transparent insect-proof self-repairing fire-retardant coating for ancient buildings, characterized by: Including amino resin, isophorone diisocyanate, ethylene-vinyl acetate copolymer, polyvinyl alcohol, phosphonitrile phosphate, guanidine phosphate, zirconium borate, pentaerythritol, phytic acid and film-forming additives; The isophorone diisocyanate is used as a curing agent for the amino resin; The isophorone diisocyanate and the amino resin are connected via a hindered urea structure; The hindered urea structure is used for self-repair and hydrogen bonding with the phytic acid.

2. A transparent insect-proof self-repairing ancient building fire-retardant coating according to claim 1, characterized in that: The film-forming additives include a thickening and leveling agent, a wetting and dispersing agent, a film-forming aid PPH, a defoaming agent and a wood stabilizer MJB-TF.

3. A transparent insect-proof self-repairing ancient building fire-retardant coating according to claim 2, characterized in that: Calculated by weight, it includes 30-40 parts of amino resin, 1-5 parts of isophorone diisocyanate, 1-5 parts of ethylene-vinyl acetate copolymer, 3-5 parts of polyvinyl alcohol, 5-10 parts of phosphonitrile phosphate, 5-10 parts of guanidine phosphate, 1-3 parts of zirconium borate, 5-10 parts of pentaerythritol, 3-6 parts of phytic acid, 0.5-1 part of thickening and leveling agent, 0.5-1 part of wetting and dispersing agent, 0.5-1 part of film-forming aid PPH, 0.5-1 part of defoaming agent and 0.5-1 part of wood stabilizer MJB-TF.

4. A method for preparing a transparent insect-proof self-repairing ancient building fire-retardant coating according to any one of claims 1 to 3, characterized in that: Initial mixing: adding amino resin, ethylene-vinyl acetate copolymer, polyvinyl alcohol, phosphonitrile phosphate, guanidine phosphate, zirconium borate, pentaerythritol and phytic acid into acetone solvent, stirring and mixing to obtain mixture A; Final mixing: adding a film-forming additive to the mixture A, adding triethanolamine to adjust the pH of the reaction step to alkaline, and then adding isophorone diisocyanate, stirring in a dark room environment, stirring evenly, and performing high-temperature curing in a dark room environment for 1 to 2 days to obtain the fire retardant coating.

5. The method for preparing a transparent insect-proof self-repairing ancient building fire-retardant coating according to claim 4, characterized in that: In the final mixing step, the pH is 8-9.

6. The method for preparing a transparent insect-proof self-repairing ancient building fire-retardant coating according to claim 5, characterized in that: In the final mixing step, the curing temperature is 70-80°C.

Citation Information

Patent Citations

  • Flame-proof liquid special for historic building and method of preparing the same

    CN101508898A

  • Waterborne transparent fireproof paint for historic buildings and preparation method of waterborne transparent fireproof paint

    CN106634394A

  • Room-temperature self-repairing water-based transparent expansion fireproof coating and preparation method thereof

    CN114250023A

  • Degradable high polymer material with main chain containing thioacetal and preparation method thereof

    CN115926165A

  • Pure bulk polymerization self-repairing elastomer and preparation method thereof

    CN118271564A