Polyurethane coating with visible light catalytic sterilization function, preparation method of polyurethane coating and electronic equipment
By introducing unsaturated double bonded photosensitive bactericides and flexible hydrophobic groups into the polyurethane coating, sterilization is achieved using visible light from electronic devices, solving the bacterial contamination and drug resistance problems on the surface of electronic devices, and achieving efficient bacterial killing and Biocompatibility.
Patent Information
- Application Number
- CN202411320341.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-20
AI Technical Summary
The prior art cannot effectively solve the problem of bacterial contamination on the surface of electronic devices, and the introduced antibacterial agents are prone to the generation of drug-resistant bacteria.
By introducing unsaturated double bonds into the polyurethane coating and combining flexible hydrophobic groups, the visible light of the electronic device itself can be used to achieve bactericidalization, avoiding the generation of drug-resistant bacteria.
Effective killing of bacteria is achieved, the biocompatibility and physical and mechanical properties of the polyurethane coating are maintained, and the generation of drug-resistant bacteria is avoided, and it has good hydrophobic properties and flexibility.
Smart Images

Figure CN119081524A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a polyurethane coating for visible light catalytic sterilization and a preparation method thereof and an electronic device, and in particular to a polyurethane coating for visible light catalytic sterilization used in electronic devices and a preparation method thereof and an electronic device having the polyurethane coating for visible light catalytic sterilization, belonging to the field of functional polymer coatings. Background Art
[0002] With the continuous development of information technology, various electronic devices have become an indispensable part of human daily life, but bacterial contamination on the surface of electronic devices has not received enough attention. Studies have shown that more than 7,000 types of bacteria have been detected on the surface of mobile phones alone. The bacterial contamination rate on the surface of mobile phones varies among different groups of people, such as: junior high school people: 66%, medical staff: 94%, and college people 96%. Nowadays, human daily life is inseparable from various electronic products, and electronic products often come into direct contact with human hands, cheeks, ears, mouths, etc. During this period, bacterial contamination on the surface of electronic products will bring serious hygiene problems and even risks of illness to humans. However, there is currently no effective method to directly solve the problem of bacterial contamination on the surface of electronic products.
[0003] Reference 1 discloses a non-migrating antibacterial coating material, which can be used to coat the inner wall of a water delivery pipeline, the inner wall of a beer and beverage storage tank, or the surface of a medical device, etc. Reference 2 discloses a photodynamic sterilization coating for the surface of an implant, wherein a hyperbranched boron-phosphorus-silicon ternary polymer is prepared by boric acid, diethyl phosphate compounds, and diethoxysilane compounds, and the polymer is sprayed on the surface of the implant to obtain a photodynamic sterilization coating. However, the preparation route of the antibacterial coating disclosed above is cumbersome and the material cost is high, which hinders the possibility of its practical application.
[0004] Reference 3 discloses an antibacterial coating of copper-based hollow titanium dioxide spheres, wherein the antibacterial coating comprises copper, copper oxide and titanium dioxide. However, the preparation process of the antibacterial coating is complicated and may also cause heavy metal pollution.
[0005] Reference 4 discloses a method for preparing a multifunctional waterborne polyurethane-monoquaternary ammonium salt polymer, which comprises mixing polyol, dibasic alcohol and polyisocyanate, reacting for a period of time under the effect of a quaternary ammonium salt catalyst, then successively adding a certain amount of chain extender, hydroxyl-containing unsaturated monomers and tertiary amine to react and obtain an isocyanate group-terminated polyurethane prepolymer, then prepolymer and the quaternary ammonium salt containing unsaturated groups are mixed in a certain mol ratio, and finally obtaining polyurethane-monoquaternary ammonium salt polymer under the effect of an oxidation-reduction initiator. But monoquaternary ammonium salt has certain cytotoxicity, and because it has been used as a bactericide for a long time, it causes problems such as microorganisms producing drug resistance and sterilization efficiency reduction.
[0006] Reference 5 discloses a method for preparing a polyurethane antibacterial nanosilver coating, in which nanosilver is attached to the surface of polyurethane by self-polymerization of dopamine to obtain an antibacterial polyurethane. However, the surface of the polyurethane loaded with silver particles is very prone to agglomeration of nanosilver, which affects the dispersion and use effect of the nanosilver.
[0007] It can be seen that although some research has been conducted on antibacterial coatings in this field, the research on antibacterial coatings that can truly be applied to the surface of smart devices to isolate bacterial contamination and will not produce drug-resistant bacteria cannot be said to be sufficient, and there is room for further research.
[0008] References:
[0009] Reference 1: CN108117831A
[0010] Reference 2: CN115737923A
[0011] Reference 3: CN115820020A
[0012] Reference 4: CN102604002A
[0013] Reference 5: CN107583112A Summary of the invention
[0014] Problem that the invention aims to solve
[0015] As mentioned above, polyurethane coating has the characteristics of good biocompatibility and excellent physical and mechanical properties, but it does not have antibacterial properties and is easily adhered by microorganisms such as bacteria and fungi. In order to give it antibacterial properties, the prior art has adopted methods such as introducing monoquaternary ammonium salts and silver particles into polyurethane, but these methods all have certain problems.
[0016] In order to solve the above problems, the present invention provides a polyurethane coating for visible light catalytic sterilization, in which a photosensitive bactericide is introduced into the polyurethane coating through an unsaturated double bond, so as to achieve visible light catalytic sterilization of the polyurethane coating, and the visible light emitted by the electronic device itself can be used to achieve the purpose of sterilization, and can be applied to the surface of the electronic device to isolate bacterial contamination. In addition, the introduction of flexible hydrophobic groups of polysiloxane can increase flexibility, thereby alleviating the problem of increased stress and unfavorable film formation caused by the introduction of reactive large steric hindrance photosensitizers into polymer chains. At the same time, the polyurethane coating of the present invention will not produce drug-resistant bacteria while having a strong bactericidal effect.
[0017] Furthermore, the present invention also provides a method for preparing a polyurethane coating for visible light catalytic sterilization. The preparation method adopts a solvent thermal volatilization method, which is simple to operate, has a wide source of raw materials, is easy to obtain, and is low in price. The obtained polyurethane coating can avoid the generation of drug-resistant bacteria and has practical application value.
[0018] In addition, the present invention also provides an electronic device having the above-mentioned visible light catalytic sterilization polyurethane coating, which can achieve the purpose of sterilization by utilizing the visible light generated by the electronic device itself.
[0019] Solutions for solving problems
[0020] [1] The present invention first provides a polyurethane coating for visible light catalytic sterilization, wherein the raw materials for preparing the polyurethane coating include functionalized polyol polymer and polyisocyanate;
[0021] The functionalized polyol polymer has structural units derived from (A) a photosensitive bactericide containing an unsaturated double bond and (B) a polymerizable monomer, and at least one of the (B) polymerizable monomers contains a hydroxyl group;
[0022] The (B) polymerizable monomers include at least (meth)acrylate monomers, and the (meth)acrylate monomers include at least (meth)acrylate monomers modified by hydrophobic substances;
[0023] Optionally, the (B) polymerizable monomer further comprises one or more olefin monomers;
[0024] The molar ratio of the (A) photosensitive bactericide containing unsaturated double bonds to the (B) polymerizable monomer is 1:8 to 1:19.
[0025] [2] According to the polyurethane coating described in [1] of the present invention, the (A) photosensitive bactericidal agent containing unsaturated double bonds includes one or more combinations of porphyrin derivatives, dihydrochlorin compounds, condensed ring quinone compounds, phthalocyanine compounds, and phenothiazine compounds.
[0026] [3] The polyurethane coating according to the present invention [1] or [2], wherein the (meth)acrylate monomer further includes a (meth)acrylate monomer containing a hydroxyl group.
[0027] [4] The polyurethane coating according to any one of [1] to [3] of the present invention, wherein the olefin monomer comprises one or more of aliphatic olefins and aromatic olefins.
[0028] [5] According to the polyurethane coating described in [4] of the present invention, the hydrophobic substance modified (meth)acrylate monomer comprises a combination of one or more of polysiloxane modified (meth)acrylate monomers or fluoropolyether alcohol modified (meth)acrylate monomers; preferably, the polysiloxane modified (meth)acrylate monomer is selected from polydimethylsiloxane-(meth)acrylate, and the fluoropolyether alcohol modified (meth)acrylate monomer is selected from perfluoropolyether alcohol-(meth)acrylate.
[0029] [6] The polyurethane coating according to [4] or [5] of the present invention, wherein the content of the polysiloxane-modified (meth)acrylate monomer in the (B) polymerizable monomer is 5 mol% to 12 mol%.
[0030] [7] The polyurethane coating according to any one of [1] to [6] of the present invention is formed in the presence of (C) an initiator, and the molar ratio of the (A) photosensitive bactericidal agent containing an unsaturated double bond to the initiator is 1:1 to 5:1.
[0031] [8] The polyurethane coating according to any one of [1] to [7] of the present invention, wherein the molar ratio of the functionalized polyol polymer to the polyisocyanate is 2:1 to 1:2.
[0032] [9] The polyurethane coating according to any one of [1] to [8] of the present invention, wherein the polyisocyanate comprises one or more of an aliphatic polyisocyanate, an alicyclic polyisocyanate and an aromatic polyisocyanate.
[0033]
[10] Furthermore, the present invention also provides a method for preparing the polyurethane coating according to any one of [1] to [9] of the present invention, comprising the following steps:
[0034] The (A) photosensitive bactericide containing an unsaturated double bond and the (B) polymerizable monomer are polymerized under the action of the (C) initiator to obtain the functionalized polyol polymer;
[0035] The functionalized polyol polymer, polyisocyanate and organic solvent are mixed and subjected to solvent thermal volatilization to obtain a polyurethane coating.
[0036]
[11] According to the preparation method described in
[10] of the present invention, the polymerization reaction temperature is 70 to 90°C and the reaction time is 3 to 24 hours.
[0037]
[12] According to the preparation method described in
[10] or
[11] of the present invention, the temperature of thermal volatilization of the solvent is 60-100°C and the time is 6-12 hours.
[0038]
[13] In addition, the present invention also provides an electronic device, which includes a display device, wherein a surface of a display element of the display device has a polyurethane coating according to any one of [1] to [9] of the present invention.
[0039] Effects of the Invention
[0040] By implementing the above technical solution, the present invention can achieve the following technical effects:
[0041] 1) The present invention introduces a photosensitive bactericide into the polyurethane coating through unsaturated double bonds, thereby achieving visible light catalytic sterilization of the polyurethane coating. The visible light emitted by the electronic device itself can be used to achieve the purpose of sterilization, and can be applied to the surface of electronic equipment to isolate bacterial contamination.
[0042] 2) The photosensitive fungicide of the present invention generates reactive oxygen species (ROS) after being irradiated with visible light. These ROS can generate oxygen-containing free radicals such as superoxide anions (O2· - ), hydroxyl radicals (·OH), or by transferring energy to surrounding oxygen molecules to form singlet oxygen molecules ( 1 O2), this sterilization method based on various visible light-excited π-conjugated photosensitizers is easy to implement and operate. In addition, ROS kills bacteria by destroying the cell membrane of bacteria and leaking cytoplasmic components, destroying DNA in the cell matrix. The polyurethane coating capable of photocatalytic sterilization of the present invention has a strong sterilization effect and will not produce drug-resistant bacteria.
[0043] 3) The raw materials for preparing the polyurethane coating of the present invention also include a flexible hydrophobic substance polysiloxane-modified (meth)acrylate monomer, and the hydrophobic substance is introduced into the coating through unsaturated double bonds, so that the polyurethane coating has good hydrophobic properties and flexibility while having bactericidal properties, which is further conducive to deposition and film formation and prevents the growth of bacteria.
[0044] 4) The present invention prepares a polyurethane coating for visible light catalytic sterilization by solvent thermal volatilization method. The preparation method is simple, the raw material source is wide, easy to obtain, and low in price. The obtained polyurethane coating can avoid the generation of drug-resistant bacteria and has practical application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 The synthetic route of the functionalized polyol polymer of Example 1;
[0046] Figure 2 The surface morphology of bacteria on the surface of the polyurethane coating for visible light catalytic sterilization prepared in Example 1 and the blank group;
[0047] Figure 3Live / dead staining of bacteria on the surface of the polyurethane coating for visible light catalytic sterilization prepared in Example 1 and the blank group;
[0048] Figure 4 The polyurethane material with visible light catalytic sterilization prepared in Example 1 was used for skin wound repair in SD rats and compared with the blank group. DETAILED DESCRIPTION
[0049] The following is a detailed description of the present invention. The following description of the technical features is based on representative embodiments and specific examples of the present invention, but the present invention is not limited to these embodiments and specific examples. It should be noted that:
[0050] In this specification, the numerical range expressed using "a numerical value A to a numerical value B" means a range including the endpoints numerical values A and B.
[0051] In the present specification, a numerical range expressed using "above" or "below" means a numerical range including the number.
[0052] In this specification, the word "may" means both performing a certain process and not performing a certain process.
[0053] In this specification, the use of "optional" or "optional" indicates that certain substances, components, execution steps, application conditions and other factors are used or not used.
[0054] In this specification, the "normal temperature" or "room temperature" used means an indoor ambient temperature of "23±2°C", and, unless otherwise specified, the "viscosity" of the present invention refers to the viscosity at this temperature.
[0055] In this specification, the unit names used are all international standard unit names, and unless otherwise stated, the "%" used indicates weight or mass percentage.
[0056] In the present specification, the use of "substantially" means that the standard deviation from a theoretical model or theoretical data is within a numerical range of 5%, preferably 3%, and more preferably 1%.
[0057] In this specification, when the terms “include” and / or “comprise” are used, they indicate the existence of features, steps, operations, devices, components and / or their combinations.
[0058] In this specification, the references to "some specific / preferred embodiments", "other specific / preferred embodiments", "embodiments", etc., mean that the specific elements (e.g., features, structures, properties and / or characteristics) described in connection with the embodiments are included in at least one embodiment described herein, and may or may not exist in other embodiments. In addition, it should be understood that the elements may be combined in various embodiments in any suitable manner.
[0059] The present invention provides a polyurethane coating for visible light catalytic sterilization and a preparation method thereof. The polyurethane coating is introduced with a photosensitive bactericide through unsaturated double bonds, thereby achieving visible light catalytic sterilization of the polyurethane coating. The visible light emitted by the electronic device itself can be used to achieve the purpose of sterilization, and the polyurethane coating can be applied to the surface of the electronic device to isolate bacterial contamination. The polyurethane coating of the present invention has a strong bactericidal effect and will not produce drug-resistant bacteria.
[0060] The present invention is based on the following insights:
[0061] It is known that polyurethane coating has good biocompatibility and mechanical properties, but it does not have antibacterial properties. In order to improve its antibacterial properties, the prior art introduces methods such as monoquaternary ammonium salts and silver particles, but these methods all have certain problems. Photodynamic antibacterial is a new technology that utilizes light of a specific wavelength to irradiate photosensitizers to promote them to produce active oxygen to destroy the cytoplasmic membrane and nucleus of bacteria to achieve the antibacterial purpose. This antibacterial mode of oxidative stress will not weaken the bactericidal effect due to the evolution of bacteria, so it does not produce drug resistance, and is one of the main means to solve the problem of bacterial drug resistance. However, there are fewer reports on the preparation of antibacterial polyurethanes in combination with polyurethane coatings. The present invention not only realizes the visible light catalytic sterilization of polyurethane coatings by introducing photosensitive bactericides into polyurethane coatings, and grafting them into polyurethane molecular chains, while introducing flexible hydrophobic groups, so as to achieve the purpose of sterilization by using visible light emitted by electronic equipment itself, and can be applied to electronic equipment surfaces to isolate bacterial contamination.
[0062] <First aspect>
[0063] A first aspect of the present invention provides a polyurethane coating for visible light catalytic sterilization, wherein the raw materials for preparing the polyurethane coating include functionalized polyol polymers and polyisocyanates.
[0064] In addition, without limitation, various optional functional additive components may be used in the polyurethane coating as long as the technical effects of the present invention are not hindered.
[0065] (Functionalized Polyol Polymer)
[0066] The functionalized polyol polymer of the present invention has structural units derived from (A) a photosensitive fungicide containing an unsaturated double bond and (B) a polymerizable monomer. In principle, there is no particular limitation on the hydroxyl functionality of the functionalized polyol polymer of the present invention, and it can usually be 2 or more.
[0067] (A) Photosensitive fungicides containing unsaturated double bonds
[0068] The photosensitive bactericide containing unsaturated double bonds can generate active oxygen under the condition of visible light excitation, and the active oxygen destroys the cell membrane of bacteria and then leaks cytoplasmic components, destroying the DNA in the cell matrix to achieve the effect of killing bacteria. At the same time, the unsaturated double bonds are polymerized with polymerizable monomers and grafted into polyol polymers to achieve the functionalization of polyol polymers.
[0069] The types of the photosensitive fungicide containing unsaturated double bonds may include one or more combinations of porphyrin derivatives, dihydrochlorin compounds, condensed ring quinone compounds, phthalocyanine compounds, and phenothiazine compounds. Among them, from the perspective of absorption wavelength, porphyrin derivatives are preferred. In some specific embodiments, the porphyrin derivatives may include tetraphenylporphyrin chloride as shown in formula (1).
[0070]
[0071] (B) polymerizable monomer
[0072] The polymerizable monomers include at least (meth)acrylate monomers. In order to improve the hydrophobicity of the polyurethane coating, prevent the growth of bacteria in a humid state, and further improve the antibacterial effect, so as to obtain a polyurethane coating that is both bactericidal and hydrophobic, the (meth)acrylate monomers include at least (meth)acrylate monomers modified by hydrophobic substances.
[0073] In some specific embodiments, the hydrophobic substance modified (meth)acrylate monomer includes a combination of one or more of polysiloxane modified (meth)acrylate monomers or fluoropolyether alcohol modified (meth)acrylate monomers; wherein the polysiloxane modified (meth)acrylate monomer can be selected from polydimethylsiloxane-(meth)acrylate and the like, and the fluoropolyether alcohol modified (meth)acrylate monomer can be selected from perfluoropolyether alcohol-(meth)acrylate and the like.
[0074] In some preferred embodiments, from the perspective of hydrophobicity and molecular chain flexibility, the (meth)acrylate monomer modified by the hydrophobic substance can be selected from the (meth)acrylate monomer modified by polysiloxane. By introducing the polysiloxane group, during the film formation process, the internal stress caused by the large steric hindrance group in the above-mentioned reactive photosensitive bactericide can be alleviated, and the final coating can also obtain a satisfactory contact angle.
[0075] In the present invention, at least one polymerizable monomer contains a hydroxyl group. In principle, there is no particular limitation on the polymerizable monomer containing a hydroxyl group, and it can be selected as needed. For example, it can be a (meth)acrylate monomer containing a hydroxyl group, or it can be an olefin monomer containing a hydroxyl group as described below. In some specific embodiments, it can include one or more combinations of hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, etc.
[0076] In some more specific embodiments, in addition to the above-mentioned polysiloxane-modified (meth)acrylate monomers and hydroxyl-containing (meth)acrylate monomers, the present invention may also include other (meth)acrylate monomers, which may include a combination of one or more of methyl methacrylate, ethyl methacrylate, etc.
[0077] Optionally, from the perspective of improving the strength and flexibility of the polyurethane coating, the polymerizable monomer also includes one or more olefin monomers. As described above, these monomers may further have or not have hydroxyl groups. In some preferred embodiments, they may include one or more aliphatic olefins (without hydroxyl groups) and aromatic olefins. Specifically, the aliphatic olefins may include a combination of one or more of ethylene, isobutylene, isoprene, etc., and the aromatic olefins may include styrene, etc.
[0078] In the present invention, the polyurethane coating layer may be formed in the presence of (C) a photoinitiator.
[0079] (C) Photoinitiator
[0080] The initiator of the present invention is a free radical initiator, which is used to make the photosensitive bactericide containing unsaturated double bonds and the polymerizable monomer undergo free radical polymerization.
[0081] The free radical initiator can be an initiator commonly used in the art, such as an azo initiator, an inorganic peroxide initiator, etc., and examples thereof include one or more of azobisisobutyronitrile (AIBN), azobisisoheptanenitrile, potassium persulfate, sodium persulfate or ammonium persulfate.
[0082] Composition of functionalized polyol polymers
[0083] The molar ratio of (A) the photosensitive bactericidal agent containing an unsaturated double bond to (B) the polymerizable monomer may be 1:8 to 1:19, for example, 1:9, 1:10, 1:12, 1:14, 1:16, 1:18, etc.
[0084] In the (B) polymerizable monomer, the content of the polysiloxane-modified (meth)acrylate monomer may be 5 mol% to 12 mol%, for example, 6 mol%, 7 mol%, 8 mol%, 9 mol%, 10 mol%, 11 mol%, etc.
[0085] The molar ratio of the photosensitive bactericide (A) containing an unsaturated double bond to the initiator (C) can be 1:1 to 5:1, such as 2:1, 2.5:1, 3:1, 3.5:1, 4:1, etc. If the initiator content is too high, the molecular weight of the functionalized polyol may be reduced, thereby affecting the surface properties of the coating. If the initiator content is too low, the purpose of the present invention may not be achieved.
[0086] (Polyisocyanate)
[0087] There is no particular limitation on the type of polyisocyanate of the present invention. Polyisocyanates commonly used in the art can be used, such as one or more of aliphatic polyisocyanates, alicyclic polyisocyanates and aromatic polyisocyanates.
[0088] The functionality of the polyisocyanate of the present invention may generally be 2 or more, and preferably 2 to 4.
[0089] The aliphatic polyisocyanate may generally be an aliphatic polyisocyanate having a linear or branched structure, such as hexamethylene diisocyanate, polyhexamethylene diisocyanate, and the like.
[0090] The alicyclic polyisocyanate may generally be a polyisocyanate having one or more aliphatic rings of four or more carbon atoms in the molecular structure, such as methylene dicyclohexyl diisocyanate or hydrogenated MDI (HMDI) and isophorone diisocyanate (IPDI).
[0091] The aromatic polyisocyanate may generally be a polyisocyanate having a benzene ring structure, for example, methylene diphenyl diisocyanate (MDI) and toluene diisocyanate (TDI).
[0092] In some preferred embodiments, the polyisocyanate of the present invention may be polyhexamethylene diisocyanate.
[0093] (Composition of polyurethane)
[0094] The polyurethane coating of the present invention can be obtained by reacting the above-mentioned functionalized polyol polymer with polyisocyanate.
[0095] In addition to the functionalized polyol polymer and polyisocyanate described above, the present invention may optionally use other required components, for example, small molecule polyols, and monoalcohols and monoisocyanates as end-capping agents.
[0096] In principle, there is no particular limitation on the ratio of the functionalized polyol polymer to the polyisocyanate, and the ratio may be 2:1 to 1:2, such as 1.5:1, 1:1, 1:1.5, and the like.
[0097] <Second Aspect>
[0098] The second aspect of the present invention provides a method for preparing the polyurethane coating for visible light catalytic sterilization according to the first aspect, comprising the following steps:
[0099] The (A) photosensitive bactericide containing an unsaturated double bond and the (B) polymerizable monomer are polymerized under the action of the (C) initiator to obtain a functionalized polyol polymer;
[0100] The functionalized polyol polymer, polyisocyanate and organic solvent are mixed and subjected to solvent thermal volatilization to obtain a polyurethane coating.
[0101] The types and amounts of the photosensitive bactericide containing unsaturated double bonds, polymerizable monomers, initiators and polyisocyanates are the same as those in the first aspect and will not be described in detail here.
[0102] The step of the polymerization reaction may specifically include: dissolving the photosensitive bactericide containing unsaturated double bonds and polymerizable monomers in an organic solvent, and then performing a polymerization reaction in the presence of an initiator.
[0103] The temperature and time of the polymerization reaction are not particularly limited and can be selected according to the temperature and time required for the initiator to initiate the reaction. In some specific embodiments, the polymerization reaction temperature is 70 to 90°C, such as 75°C, 80°C, 85°C, etc.; the polymerization reaction time is 3 to 24 hours, such as 6 hours, 10 hours, 15 hours, 20 hours, etc.
[0104] In some more specific embodiments, in order to improve the purity of the product, the polymerization reaction can be carried out under nitrogen protection.
[0105] The organic solvent may be selected from one or a combination of tetrahydrofuran, toluene, N,N-dimethylformamide, butanol, acetone and xylene.
[0106] There is no particular limitation on the amount of the organic solvent used in the polymerization reaction, and it can be selected as needed. In some specific embodiments, the molar concentration of the photosensitive bactericide containing unsaturated double bonds in the organic solvent can be 0.05 mol / L to 0.1 mol / L.
[0107] In some specific embodiments, after the polymerization reaction, the following steps are also included: removing excess solvent by rotary evaporation and then precipitating to obtain a crude polyol polymer; then dissolving the obtained crude polyol polymer in an organic solvent and then precipitating it in a precipitant; the precipitation is repeated 3 to 5 times; and then the crude polyol polymer after repeated precipitation is dried in a vacuum drying oven at 80°C for 12 hours to obtain a functionalized polyol polymer.
[0108] The precipitant is not particularly limited and can be selected as needed, for example, it can be selected from a combination of one or more of petroleum ether, n-hexane, etc.
[0109] In some specific embodiments, the amount of organic solvent used in the solvent thermal volatilization step can be expressed as 30 to 70 g / L by the mass concentration of the functionalized polyol polymer, for example, 40 g / L, 50 g / L, 60 g / L, etc.
[0110] In some specific embodiments, the temperature of the solvent thermal volatilization is 60-100°C, for example, 70°C, 80°C, 90°C, etc.; the time of the solvent thermal volatilization is 6-12h, for example, 7h, 8h, 9h, 10h, 11h, etc.
[0111] In some more specific embodiments, the solvent volatilization step can be carried out by coating a mixture of functionalized polyol polymer, polyisocyanate and organic solvent on the surface of the substrate. There is no particular limitation on the material of the substrate, and specifically, it can be selected from metal, wood, glass, etc.
[0112] <Third Aspect>
[0113] A third aspect of the present invention provides an electronic device, comprising a display device, wherein a surface of a display element of the display device has the polyurethane coating according to the first aspect.
[0114] Example
[0115] The embodiments of the present invention will be described in detail below in conjunction with the examples, but those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. If no specific conditions are specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0116] Example 1
[0117] (1) Preparation of functionalized polyol polymers:
[0118] Hydroxyethyl methacrylate (HEMA, 0.6mmol), methyl methacrylate (MMA, 0.1mmol), ethyl methacrylate (BMA, 0.1mmol), styrene (0.1mmol), tetraphenylporphyrin chloride (0.05mmol), polydimethylsiloxane-methacrylate (0.05mmol) were dissolved in 1mL of mixed solvent (toluene / butanol: 1:1). AIBN (0.03mmol) was added as an initiator under nitrogen atmosphere and stirred at 80℃ for 6h to obtain a mixed solution. After the reaction, the mixed solution was rotary evaporated to remove the residual solvent to obtain a crude polyol solution, and then the crude polyol solution was dropped into 5mL of n-hexane for precipitation. It was then redissolved in acetone and precipitated in n-hexane, and this was repeated three times. After drying, a functionalized polyol polymer was obtained.
[0119] (2) Preparation of polyurethane coating:
[0120] Weigh 0.2g of functionalized polyol polymer and 0.1g of polyhexamethylene diisocyanate (HDIT) and dissolve them in 3mL of butanone solution to obtain a mixed solution. Pipette 0.5mL of the mixed solution and apply it on the surface of substrates of different materials and place it in an oven at 60℃ for 6h to obtain a photocatalytic bactericidal polyurethane coating.
[0121] Example 2
[0122] (1) Preparation of functionalized polyol polymers:
[0123] Hydroxyethyl methacrylate (HEMA, 0.5mmol), methyl methacrylate (MMA, 0.2mmol), ethyl methacrylate (BMA, 0.1mmol), styrene (0.1mmol), tetraphenylporphyrin chloride (0.05mmol), polydimethylsiloxane-methacrylate (0.05mmol) were dissolved in 1mL of mixed solvent (toluene / butanol: 1:1). AIBN (0.03mmol) was added as an initiator under nitrogen atmosphere and stirred at 80℃ for 6h to obtain a mixed solution. After the reaction, the mixed solution was rotary evaporated to remove the residual solvent to obtain a crude polyol solution, and then the crude polyol solution was dropped into 5mL of n-hexane for precipitation. It was then redissolved in acetone and precipitated in n-hexane, and this was repeated three times. After drying, a functionalized polyol polymer was obtained.
[0124] (2) Preparation of polyurethane coating:
[0125] Weigh 0.2g of functionalized polyol polymer and 0.1g of polyhexamethylene diisocyanate (HDIT) and dissolve them in 3mL of butanone solution to obtain a mixed solution. Pipette 0.5mL of the mixed solution and apply it on the surface of substrates of different materials and place it in an oven at 60℃ for 6h to obtain a photocatalytic bactericidal polyurethane coating.
[0126] Example 3
[0127] (1) Preparation of functionalized polyol polymers:
[0128] Hydroxyethyl methacrylate (HEMA, 0.5mmol), methyl methacrylate (MMA, 0.1mmol), ethyl methacrylate (BMA, 0.2mmol), styrene (0.1mmol), tetraphenylporphyrin chloride (0.05mmol), polydimethylsiloxane-methacrylate (0.05mmol) were dissolved in 1mL of mixed solvent (toluene / butanol: 1:1). AIBN (0.03mmol) was added as an initiator under nitrogen atmosphere and stirred at 80℃ for 6h to obtain a mixed solution. After the reaction, the mixed solution was rotary evaporated to remove the residual solvent to obtain a crude polyol solution, and then the crude polyol solution was dropped into 5mL of n-hexane for precipitation. It was then redissolved in acetone and precipitated in n-hexane, and this was repeated three times. After drying, a functionalized polyol polymer was obtained.
[0129] (2) Preparation of polyurethane coating:
[0130] Weigh 0.2g of functionalized polyol polymer and 0.1g of polyhexamethylene diisocyanate (HDIT) and dissolve them in 3mL of butanone solution to obtain a mixed solution. Pipette 0.5mL of the mixed solution and apply it on the surface of substrates of different materials and place it in an oven at 60℃ for 6h to obtain a photocatalytic bactericidal polyurethane coating.
[0131] Example 4
[0132] (1) Preparation of functionalized polyol polymers:
[0133] Hydroxyethyl methacrylate (HEMA, 0.5mmol), methyl methacrylate (MMA, 0.1mmol), ethyl methacrylate (BMA, 0.1mmol), styrene (0.2mmol), tetraphenylporphyrin chloride (0.05mmol), polydimethylsiloxane-methacrylate (0.05mmol) were dissolved in 1mL of mixed solvent (toluene / butanol: 1:1). AIBN (0.03mmol) was added as an initiator under nitrogen atmosphere and stirred at 80℃ for 6h to obtain a mixed solution. After the reaction, the mixed solution was rotary evaporated to remove the residual solvent to obtain a crude polyol solution, and then the crude polyol solution was dropped into 5mL of n-hexane for precipitation. It was then redissolved in acetone and precipitated in n-hexane, and this was repeated three times. After drying, a functionalized polyol polymer was obtained.
[0134] (2) Preparation of polyurethane coating:
[0135] Weigh 0.2g of functionalized polyol polymer and 0.1g of polyhexamethylene diisocyanate (HDIT) and dissolve them in 3mL of butanone solution to obtain a mixed solution. Pipette 0.5mL of the mixed solution and apply it on the surface of substrates of different materials and place it in an oven at 60℃ for 6h to obtain a photocatalytic bactericidal polyurethane coating.
[0136] Example 5
[0137] (1) Preparation of functionalized polyol polymers:
[0138] Hydroxyethyl methacrylate (HEMA, 0.6mmol), methyl methacrylate (MMA, 0.05mmol), ethyl methacrylate (BMA, 0.05mmol), styrene (0.1mmol), tetraphenylporphyrin chloride (0.1mmol), polydimethylsiloxane-methacrylate (0.1mmol) were dissolved in 1mL of mixed solvent (toluene / butanol: 1:1). AIBN (0.03mmol) was added as an initiator under nitrogen atmosphere and stirred at 80℃ for 6h to obtain a mixed solution. After the reaction, the mixed solution was rotary evaporated to remove the residual solvent to obtain a crude polyol solution, and then the crude polyol solution was dropped into 5mL of n-hexane for precipitation. It was then redissolved in acetone and precipitated in n-hexane, and this was repeated three times. After drying, a functionalized polyol polymer was obtained.
[0139] (2) Preparation of polyurethane coating:
[0140] Weigh 0.2g of functionalized polyol polymer and 0.1g of polyhexamethylene diisocyanate (HDIT) and dissolve them in 3mL of butanone solution to obtain a mixed solution. Pipette 0.5mL of the mixed solution and apply it on the surface of substrates of different materials and place it in an oven at 60℃ for 6h to obtain a photocatalytic bactericidal polyurethane coating.
[0141] Example 6
[0142] (1) Preparation of functionalized polyol polymers:
[0143] Hydroxyethyl methacrylate (HEMA, 0.6mmol), methyl methacrylate (MMA, 0.1mmol), ethyl methacrylate (BMA, 0.1mmol), styrene (0.1mmol), tetraphenylporphyrin chloride (0.05mmol), polydimethylsiloxane-methacrylate (0.05mmol) were dissolved in 1mL of mixed solvent (toluene / butanol: 1:1). AIBN (0.05mmol) was added as an initiator under nitrogen atmosphere and stirred at 80℃ for 6h to obtain a mixed solution. After the reaction, the mixed solution was rotary evaporated to remove the residual solvent to obtain a crude polyol solution, and then the crude polyol solution was dropped into 5mL of n-hexane for precipitation. It was then redissolved in acetone and precipitated in n-hexane, and this was repeated three times. After drying, a functionalized polyol polymer was obtained.
[0144] (2) Preparation of polyurethane coating:
[0145] Weigh 0.2g of functionalized polyol polymer and 0.1g of polyhexamethylene diisocyanate (HDIT) and dissolve them in 3mL of butanone solution to obtain a mixed solution. Pipette 0.5mL of the mixed solution and apply it on the surface of substrates of different materials and place it in an oven at 60℃ for 6h to obtain a photocatalytic bactericidal polyurethane coating.
[0146] Example 7
[0147] (1) Preparation of functionalized polyol polymers:
[0148] Hydroxyethyl methacrylate (HEMA, 0.6mmol), methyl methacrylate (MMA, 0.1mmol), ethyl methacrylate (BMA, 0.1mmol), styrene (0.1mmol), tetraphenylporphyrin chloride (0.05mmol), polydimethylsiloxane-methacrylate (0.05mmol) were dissolved in 1mL of mixed solvent (toluene / butanol: 1:1). AIBN (0.03mmol) was added as an initiator under nitrogen atmosphere and stirred at 80℃ for 6h to obtain a mixed solution. After the reaction, the mixed solution was rotary evaporated to remove the residual solvent to obtain a crude polyol solution, and then the crude polyol solution was dropped into 5mL of n-hexane for precipitation. It was then redissolved in acetone and precipitated in n-hexane, and this was repeated three times. After drying, a functionalized polyol polymer was obtained.
[0149] (2) Preparation of polyurethane coating:
[0150] Weigh 0.1g of functionalized polyol polymer and 0.1g of polyhexamethylene diisocyanate (HDIT) and dissolve them in 3mL of butanone solution to obtain a mixed solution. Pipette 0.5mL of the mixed solution and apply it on the surface of substrates of different materials and place it in an oven at 60℃ for 6h to obtain a photocatalytic bactericidal polyurethane coating.
[0151] Comparative Example 1
[0152] The process is basically the same as Example 1, except that polydimethylsiloxane methacrylate is not used.
[0153] Comparative Example 2
[0154] The method is basically the same as Example 1, except that tetraphenylporphyrin chloride is not included in the polyol, and a non-reactive porphyrin compound is added separately in the preparation of the polyurethane coating to form the polyurethane coating.
[0155] Comparative Example 3
[0156] The method is substantially the same as that in Example 1, except that the amount of tetraphenylporphyrin acyl chloride is reduced to one tenth of that in Example 1.
[0157] Performance Testing
[0158] 1. Sterilization performance
[0159] The polyurethane coating with visible light catalytic sterilization prepared in Example 1 was tested for its sterilization performance against Escherichia coli (E.coil) and Staphylococcus aureus (S.aureus) under conditions of no light and light, respectively. The results are as follows: Figure 2 and Figure 3 shown.
[0160] from Figure 2 and Figure 3 It can be seen that the polyurethane coating with visible light catalytic sterilization prepared in Example 1 has no sterilization effect under the condition of no light, but has a good sterilization effect under the condition of light. Under the catalytic condition of visible light, the surface morphology of bacteria on the surface of the coating in the experimental group was damaged, and fluorescent staining showed that all bacteria were inactivated.
[0161] 2. Animal experiments
[0162] Mouse experimental steps: After SD rats were anesthetized, their backs were shaved and then depilated and disinfected, and then a 2.0 cm long incision was made on the skin. The wound was covered with a circular blank group with a diameter of 2.5 cm and an experimental group of polyurethane materials with visible light catalytic sterilization (this material has good sterilization performance) as the sample group, and the blank group was not treated in any way. In order to prevent SD rats from being irradiated to death under high-power xenon lamps, SD rats were wrapped with tin foil to expose only the wound part, and holes were punched in the tin foil under the head to leave breathing holes. The wounds of SD rats covered with materials were irradiated with a xenon lamp for 20 minutes. During the experimental observation period, all animals were fed normally, and strict aseptic operation was performed during the operation. Daily observation was performed after the operation to evaluate the infection and healing of the wound, with special attention to the observation of whether the wound had ulcers, delayed healing, suppurative infection, and inflammatory exudation. Photos were taken on the 2nd, 4th, 6th, 10th and 12th days of wound treatment to compare the wound area and healing. End point of animal experiment: The end point of this experiment was 14 days after the wound surface of SD rats recovered.
[0163] The polyurethane material prepared in Example 1 for visible light catalytic sterilization and the blank group were applied to the skin wounds of mice under dark and light conditions, respectively. The results are as follows: Figure 4 shown.
[0164] from Figure 4 It can be seen that the visible light catalytic sterilization polyurethane material prepared in Example 1 heals the fastest under light conditions and can be healed in 12 days.
[0165] 3. Hydrophobicity
[0166] The hydrophobicity of the sample was tested by measuring the contact angle. The contact angle was measured by dropping 5 μL of water on the surface of the polyurethane coating prepared in Examples 1 to 7 using a German dataphysics contact angle measuring instrument OCA15EC. The results are shown in Table 1.
[0167] 4. Antibacterial
[0168] The antibacterial effects of the polyurethane samples prepared in Examples 1 to 7 on Escherichia coli and Staphylococcus aureus were tested by the plate coating method. The results are shown in Table 1.
[0169] Table 1 Performance test results of the visible light catalytic antibacterial polyurethane coating of Examples 1 to 7
[0170] <![CDATA[Contact angle( o )]]> Antimicrobial Example 1 112 excellent Example 2 108 excellent Example 3 110 excellent Example 4 105 excellent Example 5 110 excellent Example 6 103 good Example 7 100 good Comparative Example 1 55 Difference Comparative Example 2 110 Difference Comparative Example 3 109 Difference
[0171] It can be seen from Table 1 that the polyurethane coating capable of photocatalytic sterilization of Examples 1 to 7 of the present invention has good hydrophobicity and antibacterial properties.
[0172] It can be seen from the comparison between Example 1 and Comparative Example 1 that when polydimethylsiloxane-methacrylate is not used, the polyurethane coating not only fails to obtain hydrophobicity, but also has a poor antibacterial effect.
[0173] It can be seen from the comparison between Example 1 and Comparative Example 2 that the addition of the non-reactive porphyrin compound cannot provide the polyurethane coating with good antibacterial properties, and exhibits a poor antibacterial effect.
[0174] It can be seen from the comparison between the embodiment and comparative example 3 that the content of tetraphenylporphyrin acyl chloride is too low to provide antibacterial properties for the polyurethane coating, and exhibits a poor antibacterial effect.
[0175] It should be noted that, although the technical solution of the present invention is introduced with specific examples, those skilled in the art will appreciate that the present invention should not be limited thereto.
[0176] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and variations will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or technical improvements in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.
Claims
1. A polyurethane coating for visible light catalytic sterilization, characterized in that: The raw materials for preparing the polyurethane coating include functionalized polyol polymer and polyisocyanate; The functionalized polyol polymer has structural units derived from (A) a photosensitive bactericide containing an unsaturated double bond and (B) a polymerizable monomer, and at least one of the (B) polymerizable monomers contains a hydroxyl group; The (B) polymerizable monomers include at least (meth)acrylate monomers, and the (meth)acrylate monomers include at least (meth)acrylate monomers modified by hydrophobic substances; Optionally, the (B) polymerizable monomer further comprises one or more olefin monomers; The molar ratio of the (A) photosensitive bactericide containing unsaturated double bonds to the (B) polymerizable monomer is 1:8 to 1:
19.
2. The polyurethane coating according to claim 1, characterized in that The (A) photosensitive fungicide containing unsaturated double bonds includes one or more combinations of porphyrin derivatives, dihydrochlorin compounds, condensed ring quinone compounds, phthalocyanine compounds, and phenothiazine compounds.
3. The polyurethane coating according to claim 1 or 2, characterized in that: The (meth)acrylate monomer further includes a (meth)acrylate monomer containing a hydroxyl group.
4. The polyurethane coating according to any one of claims 1 to 3, characterized in that: The olefin monomers include one or more of aliphatic olefins and aromatic olefins.
5. The polyurethane coating according to claim 4, characterized in that The hydrophobic substance modified (meth)acrylate monomer includes one or more combinations of polysiloxane modified (meth)acrylate monomers or fluoropolyether alcohol modified (meth)acrylate monomers; preferably, the polysiloxane modified (meth)acrylate monomer is selected from polydimethylsiloxane-(meth)acrylate, and the fluoropolyether alcohol modified (meth)acrylate monomer is selected from perfluoropolyether alcohol-(meth)acrylate.
6. The polyurethane coating according to claim 4 or 5, characterized in that: In the (B) polymerizable monomer, the content of the polysiloxane-modified (meth)acrylate monomer is 5 mol % to 12 mol %.
7. The polyurethane coating according to any one of claims 1 to 6, characterized in that: The polyurethane coating is formed in the presence of (C) an initiator, and the molar ratio of the (A) photosensitive bactericidal agent containing an unsaturated double bond to the initiator is 1:1 to 5:
1.
8. The polyurethane coating according to any one of claims 1 to 7, characterized in that: The molar ratio of the functionalized polyol polymer to the polyisocyanate is 2:1 to 1:
2.
9. The polyurethane coating according to any one of claims 1 to 8, characterized in that: The polyisocyanate includes one or more of aliphatic polyisocyanate, alicyclic polyisocyanate and aromatic polyisocyanate.
10. A method for preparing a polyurethane coating according to any one of claims 1 to 9, characterized in that: The following steps are involved: The (A) photosensitive bactericide containing an unsaturated double bond and the (B) polymerizable monomer are polymerized under the action of the (C) initiator to obtain the functionalized polyol polymer; The functionalized polyol polymer, polyisocyanate and organic solvent are mixed and subjected to solvent thermal volatilization to obtain a polyurethane coating.
11. The preparation method according to claim 10, characterized in that: The polymerization reaction temperature is 70-90° C. and the reaction time is 3-24 hours.
12. The preparation method according to claim 10 or 11, characterized in that: The temperature of the thermal volatilization of the solvent is 60-100° C. and the time is 6-12 hours.
13. An electronic device, comprising a display device, characterized in that: The display element surface of the display device has the polyurethane coating according to any one of claims 1 to 9.
Citation Information
Patent Citations
Limonene-based polyurethane with high water resistance and toluene resistance and preparation method thereof
CN106519159A
Water-soluble polymerizable photosensitive monomer, and preparation method and application thereof
CN109384684A
Nonsaturated polyol and photocurable polyurethane prepared from nonsaturated polyol and manufacturing method thereof
CN109957083A
Antibacterial polymer coating composition and antibacterial polymer film
CN112585227A
Polyurethane composition, preparation method and application thereof
CN112823174A