Packaging adhesive film, preparation method thereof and photovoltaic module

By adjusting the polar group surface density and optimization process on the surface of the packaging adhesive film, the problem of insufficient reliability of the existing adhesive film on new photovoltaic cells is solved, the peel strength and water vapor transmission rate are improved, and the packaging of photovoltaic modules is enhanced Reliability and stability.

CN119081582APending Publication Date: 2024-12-06FIRST (CHUZHOU) NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411344935.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The lack of reliability of existing packaging films on new photovoltaic cells leads to low peel strength and increased production and processing difficulty, affecting the long-term reliability of photovoltaic modules.

Method used

By adjusting the polar group surface density of the encapsulated adhesive film to 0.5-2.5 mg/cm2, combined with plasma treatment and spray treatment technology, the composition and process of the adhesive film are optimized, and the bond strength between the adhesive film and the battery cell is improved. and water vapor transmittance.

Benefits of technology

The peel strength and water vapor transmission between the packaging film and the battery cell are improved, the production cost is reduced, and the overall packaging reliability and long-term use stability of photovoltaic modules are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081582A_ABST
    Figure CN119081582A_ABST
Patent Text Reader

Abstract

The invention provides a packaging adhesive film, a preparation method thereof and a photovoltaic module. The composition of the packaging adhesive film comprises the following components in parts by weight: 100 parts of matrix resin, 0.1-2 parts of a cross-linking agent, 0.1-5 parts of a silane coupling agent and 0.1-3 parts of an auxiliary agent, wherein at least one surface of the packaging adhesive film contains polar groups, and the surface density of the polar groups is 0.5-2.5 mg / cm < 2 >; the polar group is selected from any one or more of hydroxyl, carbonyl, carboxyl, epoxy group, acylamino, siloxy and anhydride group. According to the packaging adhesive film disclosed by the invention, the surface of the packaging adhesive film is treated, so that the peeling strength of the packaging adhesive film and a battery piece is improved, and meanwhile, the comprehensive properties such as mechanical property, transparency and packaging property of the packaging adhesive film are also ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of photovoltaic modules, and in particular to a packaging adhesive film, a preparation method thereof, and a photovoltaic module. Background Art

[0002] In recent years, crystalline silicon solar cell technology has developed rapidly, and the technology iteration has been significantly accelerated. Research on new battery technologies such as tunnel oxide passivated contact solar cells (TOPCon cells), heterojunction cells (HJT cells), and perovskite cells has become more and more in-depth, and the market coverage has increased year by year. Different from the relatively mature emitter back passivated cells (PERC cells), the structure of the new battery has changed, and its surface composition and structure have been adjusted accordingly, and the requirements for related auxiliary materials have also changed accordingly.

[0003] Encapsulation film is one of the key auxiliary materials for solar cell modules. It isolates the modules from corrosion by water and oxygen, provides mechanical support, and provides strong support for the long-term reliability of crystalline silicon solar cell modules. For new battery technologies such as TOPCon cells and HJT cells, changes in surface structure cause existing conventional films adapted to PERC cells to fail reliability tests, which can easily lead to a series of reliability problems, which is not conducive to the rapid development of new battery technologies. In addition, the current encapsulation films with EVA or POE as the matrix resin have poor adhesion on new battery cells, and reliability tests are difficult to meet requirements. Therefore, the encapsulation film needs to be improved accordingly to adapt to new battery cells. Summary of the invention

[0004] The main purpose of the present invention is to provide a packaging film and a preparation method thereof and a photovoltaic module to solve the problem of low reliability of the packaging film in the photovoltaic module of the prior art.

[0005] In order to achieve the above object, according to one aspect of the present invention, a packaging film is provided. The composition of the packaging film comprises, by weight, 100 parts of a base resin, 0.1 to 2 parts of a cross-linking agent, 0.1 to 5 parts of a silane coupling agent, and 0.1 to 3 parts of an auxiliary agent; wherein the packaging film comprises polar groups on at least one surface, and the surface density of the polar groups is 0.5 to 2.5 mg / cm 2 ; The polar group is selected from any one or more of a hydroxyl group, a carbonyl group, a carboxyl group, an epoxy group, an amide group, a silane group and an anhydride group.

[0006] Furthermore, the encapsulation film comprises a first surface and a second surface, and the surface density of the polar groups on the first surface is greater than or equal to the surface density of the polar groups on the second surface; preferably, the surface density of the polar groups on the first surface is 0.5 to 2.5 mg / cm 2; The surface density of polar groups on the second surface is less than 0.5 mg / cm 2 .

[0007] Furthermore, the polar groups are silanoxy groups, and the difference between the surface density of the silanoxy groups on the first surface and the surface density of the silanoxy groups on the second surface is 0.5 to 2.5 mg / cm 2 .

[0008] Furthermore, the peel strength between the above-mentioned encapsulation film and the battery cell is 29-53 mN / m; and / or, the water vapor permeability of the encapsulation film is 3.1-3.5%; and / or, the light transmittance of the encapsulation film is 89.2-90.6%; and / or, the hardness of the encapsulation film is 55-66 HA; and / or, the melt index of the matrix resin is 1.0-30 g / 10 min; and / or, the light transmittance of the matrix resin is ≥88%; and / or, the matrix resin is selected from any one or more of ethylene-vinyl acetate copolymer, polyolefin elastomer, polyethylene, polypropylene and ethylene propylene diene monomer rubber.

[0009] According to another aspect of the present invention, a method for preparing the aforementioned encapsulating film is provided, the method comprising: subjecting at least one surface of a film prepared from a composition of the encapsulating film to surface treatment to obtain the encapsulating film; the surface treatment comprising sequentially performing plasma treatment, spray treatment and baking treatment; wherein the spray treatment solution comprises a polar group source, the mass concentration of the polar group source in the spray treatment solution is 1 to 10 wt %, the jet velocity of the spray treatment solution is 0.5 to 5 L / h, and the spray treatment time is 30 to 60 s; the polar group source is selected from any one or more of a hydroxyl source, a carbonyl source, a carboxyl source, an epoxy source, an amide source, a silaneoxy source and an anhydride source.

[0010] Furthermore, the gas for the plasma treatment is a nitrogen-containing gas, and preferably the nitrogen-containing gas is selected from any one or more of nitrogen, ammonia, nitrous oxide and nitrogen dioxide; further preferably, the nitrogen-containing gas is nitrogen; and / or the flow rate of the nitrogen-containing gas is 5 to 50 L / min.

[0011] Further, the above-mentioned hydroxyl source is hydroxyethyl methacrylate and / or hydroxyethyl acrylate; and / or, the carbonyl source is selected from any one or more of methyl methacrylate, butyl methacrylate and tert-butyl methacrylate; and / or, the carboxyl source is selected from any one or more of methacrylic acid, acrylic acid and itaconic acid; and / or, the epoxy source is glycidyl methacrylate and / or 2,3-epoxypropyl acrylate; and / or, the amide source is acrylamide and / or methacrylamide; and / or, the silaneoxy source is selected from any one or more of vinyltrimethoxysilane, vinyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane coupling agent and vinyl silane; and / or, the anhydride source is selected from any one or more of maleic anhydride, acrylic anhydride and methacrylic anhydride; and / or, the spray-treated solution also includes a solvent, and the solvent is selected from any one or more of n-hexane, ethanol, ethyl acetate, 1,2-dichloroethane, methanol and isopropanol.

[0012] Furthermore, the discharge power of the above-mentioned plasma treatment is 500-8000W; and / or the discharge gas pressure of the plasma treatment is 10-101325Pa; and / or the time of the plasma treatment is 10-50s; and / or the temperature of the baking treatment is 50-90°C; and / or the time of the baking treatment is 0.2-1.0min.

[0013] According to another aspect of the present invention, a photovoltaic module is provided, wherein the photovoltaic module contains the aforementioned packaging film.

[0014] Furthermore, the surface density of the polar groups of the encapsulation film is 0.5 to 2.5 mg / cm 2 One side surface is in contact with the battery cell.

[0015] By applying the technical solution of the present invention, the existing encapsulation film has insufficient encapsulation reliability for the new type of battery cell module. When the density of the surface polar groups of the encapsulation film is too low, the peel strength between the encapsulation film and the contact substrate is insufficient, especially the peel strength between the encapsulation film and the battery cell is insufficient, resulting in reduced reliability of the photovoltaic module in long-term use. When the density of the surface polar groups of the encapsulation film is too high, the difficulty of production and processing of the encapsulation film increases, which is not conducive to improving the production efficiency of the encapsulation film. At the same time, the adhesion between the encapsulation film and the battery cell is not improved more significantly. Moreover, the excessively high density of the polar groups may cause the water vapor barrier of the photovoltaic module to decrease, which is not conducive to the long-term reliability of the photovoltaic module. The surface density of the polar groups on at least one side of the encapsulation film is controlled to be 0.5-2.5 mg / cm 2 The polar group surface density of the encapsulating film is within the range of 0.5 to 2.5 mg / cm 2The surface on one side is arranged in contact with the battery cell, which helps to improve the intermolecular interaction force between the packaging film and the surface components of the battery cell, thereby improving the peeling strength between the packaging film and the battery cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0017] Figure 1 The process flow chart of preparing the encapsulation film in Example 1 of the present application is shown.

[0018] The above drawings include the following reference numerals:

[0019] 1. Unwinding roller; 2. Tension roller; 3. Transition roller; 4. Squeeze roller; 5. Winding roller; 6. Plasma treatment area; 7. Spray treatment area; 8. Drying area. DETAILED DESCRIPTION

[0020] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0021] As analyzed in the background technology of the present application, the photovoltaic modules in the prior art have the problem of low reliability of the encapsulation film. In order to solve the above problem, the present application provides an encapsulation film and a preparation method thereof and a photovoltaic module.

[0022] In a typical embodiment of the present application, a packaging film is provided, wherein the composition of the packaging film comprises, by weight, 100 parts of a base resin, 0.1 to 2 parts of a cross-linking agent, 0.1 to 5 parts of a silane coupling agent, and 0.1 to 3 parts of an auxiliary agent; wherein at least one surface of the packaging film contains polar groups, and the surface density of the polar groups is 0.5 to 2.5 mg / cm 2 ; The polar group is selected from any one or more of a hydroxyl group, a carbonyl group, a carboxyl group, an epoxy group, an amide group, a silane group and an anhydride group.

[0023] The existing encapsulation film has insufficient encapsulation reliability for new cell modules. When the density of the surface polar groups of the encapsulation film is too low, the peel strength between the encapsulation film and the contact substrate is insufficient, especially the peel strength between the encapsulation film and the cell is insufficient, resulting in reduced reliability of the photovoltaic module in long-term use. When the density of the surface polar groups of the encapsulation film is too high, the difficulty of production and processing of the encapsulation film increases, which is not conducive to improving the production efficiency of the encapsulation film. At the same time, the adhesion between the encapsulation film and the cell is not improved more significantly. Moreover, the high density of the polar groups may cause the water vapor barrier of the photovoltaic module to decrease, which is not conducive to the long-term reliability of the photovoltaic module. The surface density of the polar groups on at least one side of the encapsulation film is controlled to be 0.5-2.5 mg / cm 2 The polar group surface density of the encapsulating film is within the range of 0.5 to 2.5 mg / cm 2 The surface on one side is arranged in contact with the battery cell, which helps to improve the intermolecular interaction force between the packaging film and the surface components of the battery cell, thereby improving the peeling strength between the packaging film and the battery cell.

[0024] In one embodiment of the present application, the encapsulation film comprises a first surface and a second surface, and the surface density of the polar groups on the first surface is greater than or equal to the surface density of the polar groups on the second surface; preferably, the surface density of the polar groups on the first surface is 0.5 to 2.5 mg / cm 2 ; The surface density of polar groups on the second surface is less than 0.5 mg / cm 2 .

[0025] The first surface is arranged in contact with the battery cell, and the second surface is arranged in contact with the packaging front plate or the packaging back plate. If the surface density of the polar groups on the second surface is too high, the processing difficulty of the packaging film itself will increase, the cost will rise, and it will not be conducive to improving the light transmittance of the packaging film and reducing the hardness of the packaging film, but will lead to a decrease in the reliability of the photovoltaic module. It is preferred to control the surface density of the polar groups on the first surface and the surface density of the polar groups on the second surface within the above range, which helps to improve the interaction force between the packaging film and the battery cell and the packaging front plate or the packaging back plate, and avoid the risks of increased process difficulty, reduced light transmittance and increased hardness caused by excessive polar groups, thereby helping to improve the overall packaging reliability of the photovoltaic module.

[0026] In one embodiment of the present application, the polar group is a silaneoxy group, and the difference between the surface density of the silaneoxy groups on the first surface and the surface density of the silaneoxy groups on the second surface is 0.5 to 2.5 mg / cm 2 .

[0027] It is preferred to control the difference between the surface density of the silaneoxy groups on the first surface and the surface density of the silaneoxy groups on the second surface within the above range, which helps to improve the interaction force between the encapsulation film and the battery cell and the encapsulation front plate or the encapsulation back plate, and avoid the risks of increased process difficulty, reduced light transmittance and increased hardness caused by excessive polar groups, thereby helping to improve the overall encapsulation reliability of the photovoltaic module. Further, the encapsulation front plate or the encapsulation back plate is selected from glass, polymer sheets, etc. As a solution for some laminated components, the encapsulation front plate may also be other types of battery cells; most preferably, the encapsulation front plate or the encapsulation back plate is a glass sheet. The encapsulation film is used for the encapsulation of photovoltaic modules, and at least one side of the surface contacts the battery cell, and the other side of the surface contacts other surfaces. Due to the difference in the contact medium, the polar group density of the first surface and the second surface of the encapsulation film is controlled to be different, which can not only ensure the peel strength of each contact surface, but also control the production cost and optimize the production efficiency.

[0028] In one embodiment of the present application, the peel strength between the above-mentioned packaging film and the battery cell is 29-53 mN / m; and / or, the water vapor permeability of the packaging film is 3.1-3.5%; and / or, the light transmittance of the packaging film is 89.2-90.6%; and / or, the hardness of the packaging film is 55-66HA.

[0029] Since the surface density of polar groups on at least one side of the encapsulation film of the present application is 0.5-2.5 mg / cm 2 Therefore, the encapsulation film has the peel strength, water vapor permeability, light transmittance and hardness within the above ranges, and the first surface with the above peel strength is placed in contact with the battery cell, which helps to improve the packaging reliability of the photovoltaic module.

[0030] Preferably, the crosslinking agent is selected from 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, 1,1-(ditert-butylperoxy)3,3,5-trimethylcyclohexane, tert-butyl peroxybenzoate, triphenylmethane-4,4',4"-triisocyanate, diisopropyl peroxide, bis(2-tert-butylperoxyisopropyl)benzene, tert-butyl peroxide isopropyl benzene, tert-amyl peroxybenzoate, ditert-amyl peroxide, tert-butyl peroxybenzoic acid Any one or more of tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxy-3,5,5-trimethylhexanoate, di(4-chlorobenzoyl)peroxide, di(2,4-dichlorobenzyl)peroxide, di(4-methylphenyl)peroxide, n-butyl-4,4-di(tert-butylperoxy)valerate, ethyl-3,3-di(tert-butylperoxy)butyrate, and tert-butylperoxy-2-ethylhexylcarbonate;

[0031] The composition of the above-mentioned encapsulation film also includes 0 to 1 parts of a cross-linking aid; including but not limited to, the cross-linking aid is selected from any one or more of triallyl isocyanurate, triallyl cyanurate, trimethylolpropane trimethacrylate, trimethylolpropane triacrylate and pentaerythritol tetramethacrylate.

[0032] In a preferred embodiment, the silane coupling agent is selected from any one or more of vinyltrimethoxysilane, vinyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane, 3-(2,3-epoxypropoxy)propyltrimethoxysilane, methacrylate silane, and vinyltriisopropoxysilane.

[0033] When the silane coupling agent is selected from the above types, it is beneficial to increase the surface density of polar groups on the surface of the encapsulation film; the weight proportion of the silane coupling agent in the composition of the encapsulation film is 0.1 to 5 parts. When the content of the silane coupling agent in the encapsulation film is greater than 5 parts, the processing performance of the encapsulation film is reduced, and it is difficult to form a film through extrusion casting equipment.

[0034] In order to further improve the anti-aging performance of the encapsulation film, in a preferred embodiment, the antioxidant is selected from any one or more of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, n-octadecyl β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, and 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl) isocyanuric acid.

[0035] In order to further improve the anti-aging performance of the encapsulation film, in a preferred embodiment, the light stabilizer is selected from any one or more of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate, bis(1-octyloxy-2,2,6,6-tetramethyl-4-piperidinyl) sebacate, poly(4-hydroxy-2,2,6,6-tetramethyl-1-piperidinethanol) succinate, 2-hydroxy-4-n-octyloxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxy-2'-carboxybenzophenone, and 2,4-dihydroxybenzophenone.

[0036] In one embodiment of the present application, the melt flow rate of the above-mentioned matrix resin is 1.0-30g / 10min; and / or the transmittance of the matrix resin is ≥88%; and / or the matrix resin is selected from any one or more of ethylene-vinyl acetate copolymer, polyolefin elastomer, polyethylene, polypropylene and ethylene propylene diene monomer rubber.

[0037] It is preferred to control the melt flow rate of the matrix resin, the transmittance of the matrix resin and the type of the matrix resin within the above range, which helps to give full play to the synergistic effect between the components. Therefore, the encapsulation film of the present application has better comprehensive properties such as mechanical properties, transparency, and encapsulation performance.

[0038] It is preferred to control the type and number of the composition of the encapsulating film within the above range, which helps to control the surface density of polar groups on the surface of the encapsulating film and make the comprehensive performance of the encapsulating film, such as mechanical properties, transparency, and encapsulation performance, better. The addition of a crosslinking agent and a co-crosslinking agent helps to improve the crosslinking ability of the encapsulating film, a silane coupling agent helps to improve the mechanical properties of the encapsulating film, and the addition of auxiliary agents such as antioxidants and ultraviolet absorbers helps to improve the aging resistance of the encapsulating film. Since the encapsulating film of the present application is a surface treatment of the encapsulating film, the encapsulating film of the present application does not affect the comprehensive performance of the encapsulating film, such as mechanical properties, transparency, and encapsulation performance, while improving the peel strength between the encapsulating film and the battery cell.

[0039] In order to make the encapsulation film provided by the present application more widely applicable to the encapsulation of new solar cell sheets, in a preferred embodiment, the thickness of the encapsulation film is 0.01 to 1.0 mm.

[0040] Furthermore, in order to achieve a polar group surface density of 0.5 to 2.5 mg / cm on at least one side of the encapsulation film, 2 Preferably, at least one side of the surface of the encapsulating film is subjected to a grafting treatment, and the grafting treatment can be performed by using a solution having polar groups to treat the surface of the encapsulating film.

[0041] Furthermore, one side of the encapsulation film surface is processed, which can be a whole-surface treatment or a patterned treatment, such as a grid patterning, in which the corresponding battery cell portion is processed and the non-battery cell portion is not processed. At least one surface is processed, and the processed area is preferably greater than or equal to 80%, preferably greater than or equal to 90%, and more preferably 100%.

[0042] In another typical embodiment of the present application, a method for preparing the aforementioned encapsulating film is provided, the preparation method comprising: subjecting at least one surface of the encapsulating film prepared from the composition of the encapsulating film to surface treatment to obtain the encapsulating film; the surface treatment comprises plasma treatment, spray treatment and baking treatment performed in sequence; wherein the spray treatment solution contains a polar group source, the mass concentration of the polar group source in the spray treatment solution is 1 to 10 wt %, the jet velocity of the spray treatment solution is 0.5 to 5 L / h, and the spray treatment time is 30 to 60 s; the polar group source is selected from any one or more of a hydroxyl source, a carbonyl source, a carboxyl source, an epoxy source, an amide source, a silaneoxy source and an anhydride source.

[0043] The above-mentioned plasma treatment process destroys the surface molecular chains of the encapsulation film so that active groups are generated on the surface of the encapsulation film, thereby providing more active sites for the polar groups. When the spray-treated solution is sprayed on the surface of the encapsulation film, the polar groups in the spray-treated solution form covalent bonds with the active groups on the surface of the encapsulation film. After drying, the formation of covalent bonds between the polar groups and the active groups is further promoted to obtain an encapsulation film with stronger polarity. The encapsulation film with stronger polarity can have stronger molecular interactions with the surface of the battery cell, thereby helping to improve the peeling strength between the encapsulation film and the battery cell. It is preferred to control the mass concentration of the polar group source in the spray-treated solution, the jet velocity of the spray-treated solution and the spray treatment time within the above range, which helps to control the density of the polar groups in the encapsulation film finally formed, thereby helping to further improve the peeling strength between the encapsulation film and the battery cell. In addition, the preparation method of the present application has the advantages of high efficiency, rapidity and simplicity.

[0044] In addition, it is preferred that the spray treatment is performed in the vertical direction of the packaging film, and the plasma treatment gas is introduced from the middle of the plasma treatment area and overflows from both ends to ensure that the gas composition in the plasma treatment area does not change much.

[0045] In one embodiment of the present application, the gas for the above-mentioned plasma treatment is a nitrogen-containing gas, and the nitrogen-containing gas is preferably selected from any one or more of nitrogen, nitrous oxide and nitrogen dioxide; it is further preferred that the nitrogen-containing gas is nitrogen; and / or the flow rate of the nitrogen-containing gas is 5 to 50 L / min.

[0046] The gas used in the plasma treatment is preferably a nitrogen-containing gas, which helps to destroy the surface molecular chains of the packaging film during the plasma treatment process so that active nitrogen groups (such as N·, N2·, etc.) are generated on the surface of the packaging film. These groups have high reactivity and are easy to react with polar groups to form strong covalent bonds. It is preferred to control the type of nitrogen-containing gas within the above range to help improve the efficiency of the plasma treatment. Nitrogen as a gas source can generate a certain amount of nitrogen-containing active groups on the surface of the material, which helps to further increase the strength of the covalent bonds formed between the polar groups and the active groups on the surface of the packaging film.

[0047] In order to further improve the peel strength between the encapsulation film and the battery cell and reduce the cost of the solution for the spray treatment, in one embodiment of the present application, it is preferred that the above-mentioned hydroxyl source is hydroxyethyl methacrylate and / or hydroxyethyl acrylate; and / or, the carbonyl source is selected from any one or more of methyl methacrylate, butyl methacrylate and tert-butyl methacrylate; and / or, the carboxyl source is selected from any one or more of methacrylic acid, acrylic acid and itaconic acid; and / or, the epoxy source is glycidyl methacrylate and / or 2,3-epoxypropyl acrylate; and / or, the amide source is acrylamide and / or methacrylamide; and / or, the silaneoxy source is selected from any one or more of vinyltrimethoxysilane, vinyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane coupling agent and vinyl silane; and / or, the anhydride source is selected from any one or more of maleic anhydride, acrylic anhydride and methacrylic anhydride; and / or, the solution for the spray treatment also includes a solvent, and the solvent is selected from any one or more of n-hexane, ethanol, ethyl acetate, 1,2-dichloroethane, methanol and isopropanol.

[0048] In addition, the concentration of the polar group source for spray treatment may be 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt% or 10 wt%.

[0049] In order to improve the efficiency of plasma treatment, so that more activated groups are formed on the surface of the packaging film, thereby improving the polarity of the packaging film, in one embodiment of the present application, it is preferred that the discharge power of the above-mentioned plasma treatment is 500~8000W; and / or, the discharge gas pressure of the plasma treatment is 10~101325Pa; and / or, the time of the plasma treatment is 10~50s.

[0050] In addition, the plasma treatment time may be 10 s, 20 s, 30 s, 40 s or 50 s.

[0051] In order to further promote the efficiency and effect of forming covalent bonds between polar groups and active groups, in one embodiment of the present application, the baking treatment temperature is preferably 50 to 90° C.; and / or the baking treatment time is 0.2 to 1.0 min.

[0052] In another typical embodiment of the present application, a photovoltaic module is provided, wherein the photovoltaic module contains the aforementioned encapsulation film.

[0053] Since the above photovoltaic module contains the encapsulation film of the present application, the encapsulation film in the photovoltaic module has a high bonding strength with the solar cell, which helps to improve the reliability of the photovoltaic module and reduce potential induced degradation.

[0054] In order to further improve the reliability of photovoltaic modules and reduce potential induced degradation, in one embodiment of the present application, the surface density of the polar groups of the encapsulation film is preferably 0.5-2.5 mg / cm 2 One side surface is in contact with the battery cell.

[0055] The beneficial effects of the present application will be further illustrated below in conjunction with embodiments.

[0056] Example 1

[0057] In parts by weight, the composition of the encapsulation film is 100 parts of an ethylene-octene copolymer resin having a melt index of 10.0 g / 10 min, 1.0 parts of 1,1-(di-tert-butylperoxide)3,3,5-trimethylcyclohexane, 1.0 parts of triallyl isocyanurate, 2.0 parts of vinyltrimethoxysilane, 0.1 parts of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate and 0.1 parts of bis(2,2,6,6-tetramethyl-4-piperidinyl)sebacate.

[0058] Reference Figure 1 The process flow chart of the encapsulating film is shown in FIG. 1 . The encapsulating film is prepared. Specifically, the composition of the encapsulating film is mixed and the extruded film is surface treated. Specifically, the film is fixed on the unwinding roller 1, passes through the tension roller 2, and then passes through the plasma treatment area 6, the spray treatment area 7 and the baking treatment area 8 on the transition roller 3 in sequence, and then passes through the squeezing roller 4, the tension roller 2 and the winding roller 5 in sequence to obtain the encapsulating film. Among them, through the tension setting, the tension balance of the whole roll of film is achieved, the tension value is 80kg, the gas for plasma treatment is nitrogen, the flow rate of nitrogen is 25L / min, nitrogen is introduced from the middle of the plasma treatment area, and flows out from both sides, the discharge power of plasma treatment is 1000W, the time of plasma treatment is 30s, the solution for spray treatment is vinyl silane solution, the solvent is n-hexane, the concentration of vinyl silane solution is 2.0wt%, the flow rate of vinyl silane solution is 1.0L / h, the time of spray treatment is 40s, the temperature of drying treatment is 90℃, the time of drying treatment is 0.5min, and the packaging film is obtained. The polar group is silaneoxy, and the surface density of silaneoxy on the first side of the surface-treated packaging film is 1.2mg / cm 2 The difference between the surface density of the silane alkoxy groups on the second surface of the encapsulation film without surface treatment is 1.2 mg / cm 2 .

[0059] Example 2

[0060] The difference from Example 1 is that the concentration of the vinyl silane solution in the spray treatment area is 1.0wt%, the flow rate of the vinyl silane solution is 5.0L / h, and the spray treatment time is 40s. Finally, a packaging film is obtained, wherein the surface density of the silane alkoxy group on the first surface of the surface-treated packaging film is 1.6mg / cm 2 The difference between the silane oxygen density of the second surface of the encapsulation film and the surface without surface treatment is 1.6 mg / cm 2 .

[0061] Example 3

[0062] The difference from Example 1 is that the concentration of the vinyl silane solution in the spray treatment area is 5.0wt%, the flow rate of the vinyl silane solution is 3.0L / h, and the spray treatment time is 40s. Finally, a packaging film is obtained, wherein the surface density of the silane alkoxy group on the first surface of the surface-treated packaging film is 2.2mg / cm 2 The difference between the silane oxygen density of the second surface of the encapsulation film and the surface without surface treatment is 2.2 mg / cm 2 .

[0063] Example 4

[0064] The difference from Example 1 is that the concentration of the vinyl silane solution in the spray treatment area is 10.0wt%, the flow rate of the vinyl silane solution is 0.5L / h, and the spray treatment time is 30s. Finally, a packaging film is obtained, wherein the surface density of the silane alkoxy group on the first surface of the surface-treated packaging film is 1.1mg / cm 2 The difference between the silane oxygen density of the second surface of the encapsulation film and the surface without surface treatment is 1.1 mg / cm 2 .

[0065] Example 5

[0066] The difference from Example 1 is that the concentration of the vinyl silane solution in the spray treatment area is 1.0wt%, the flow rate of the vinyl silane solution is 0.5L / h, and the spray treatment time is 40s. Finally, a packaging film is obtained, wherein the surface density of the silane alkoxy group on the first surface of the surface-treated packaging film is 0.5mg / cm 2 The difference between the silane oxygen density of the second surface of the encapsulation film and the surface without surface treatment is 0.5 mg / cm 2 .

[0067] Example 6

[0068] The difference from Example 1 is that the concentration of the vinyl silane solution in the spray treatment area is 10.0wt%, the flow rate of the vinyl silane solution is 2.5L / h, and the spray treatment time is 30s. Finally, a packaging film is obtained, wherein the surface density of the silane alkoxy group on the first surface of the surface-treated packaging film is 2.5mg / cm 2 The difference between the silane oxygen density of the second surface of the encapsulation film and the surface without surface treatment is 2.5 mg / cm 2 .

[0069] Example 7

[0070] The difference from Example 1 is that the solution for spraying treatment is butyl methacrylate solution, the solvent is ethanol, and finally a packaging film is obtained, wherein the polar group is a carbonyl group, and the surface density of the carbonyl group on the first surface of the surface-treated packaging film is 1.0 mg / cm 2 The difference between the surface density of carbonyl groups on the second surface of the encapsulation film without surface treatment is 1.0 mg / cm 2 .

[0071] Example 8

[0072] The difference from Example 1 is that the weight portion of 1,1-(ditert-butylperoxide)3,3,5-trimethylcyclohexane is 2 parts, the weight portion of triallyl isocyanurate is 1 part, the weight portion of vinyl trimethoxysilane is 0.1 parts, the weight portion of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate is 1.5 parts, and the weight portion of bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate is 1.5 parts, and finally a packaging film is obtained, wherein the surface density of the silaneoxy group on the surface of the surface-treated packaging film is 1.2 mg / cm 2 The difference between the surface density of silane oxy groups and the surface density of the untreated surface is 1.2 mg / cm 2 .

[0073] Example 9

[0074] The difference from Example 1 is that the weight portion of 1,1-(ditert-butylperoxide)3,3,5-trimethylcyclohexane is 0.1 parts, the weight portion of triallyl isocyanurate is 0 parts, the weight portion of vinyl trimethoxysilane is 5 parts, the weight portion of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate is 0.05 parts, and the weight portion of bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate is 0.05 parts, and finally a packaging film is obtained, wherein the surface density of the silaneoxy group on the surface of the surface-treated packaging film is 1.0 mg / cm 2 The difference between the surface density of silane oxy groups on the surface without surface treatment is 1.0 mg / cm 2 .

[0075] Example 10

[0076] The difference from Example 1 is that the flow rate of nitrogen is 5 L / min, the discharge power of plasma treatment is 8000 W, the discharge pressure of plasma treatment is 10 Pa, the time of plasma treatment is 10 s, and finally a packaging film is obtained.

[0077] Embodiment 11

[0078] The difference from Example 1 is that the flow rate of nitrogen is 50 L / min, the discharge power of plasma treatment is 500 W, the discharge gas pressure of plasma treatment is 101325 Pa, the plasma treatment time is 50 s, and finally a packaging film is obtained.

[0079] Example 12

[0080] The difference from Example 1 is that the flow rate of nitrogen is 60 L / min, the discharge power of plasma treatment is 9000 W, the discharge pressure of plasma treatment is 5 Pa, the time of plasma treatment is 5 s, and finally a packaging film is obtained.

[0081] Embodiment 13

[0082] The difference from Example 1 is that the baking temperature is 50° C., the baking time is 1.0 min, and finally a packaging film is obtained.

[0083] Embodiment 14

[0084] The difference from Example 1 is that the baking temperature is 90° C., the baking time is 0.2 min, and finally a packaging film is obtained.

[0085] Embodiment 15

[0086] The difference from Example 1 is that no baking treatment is performed, and finally a packaging film is obtained.

[0087] Example 16

[0088] The difference from Example 1 is that after the surface treatment of the first side of the film is completed, the second side of the film is surface treated using the same process to finally obtain an encapsulation film. The surface density of the polar groups on the second side is 1.2 mg / cm 2 The difference in the surface density of the siloxane groups on the first and second surfaces is 0.0 mg / cm 2 .

[0089] Comparative Example 1

[0090] The difference from Example 1 is that the concentration of the vinyl silane solution in the spray treatment area is 12wt%, the flow rate of the vinyl silane solution is 6L / h, and the spray treatment time is 30s, and finally a packaging film is obtained. Among them, the surface density of the silane alkoxy group on the first side of the surface treated packaging film is 3.0mg / cm 2 The difference between the silane oxygen density of the second surface of the encapsulation film and the surface without surface treatment is 3.0 mg / cm 2 .

[0091] Comparative Example 2

[0092] The difference from Example 1 is that the concentration of the vinyl silane solution in the spray treatment area is 0.8wt%, the flow rate of the vinyl silane solution is 0.5L / h, and the spray treatment time is 20s. Finally, a packaging film is obtained, wherein the surface density of the silane alkoxy group on the first surface of the surface-treated packaging film is 0.1mg / cm 2 The difference between the silane oxygen density of the second surface of the encapsulation film and the surface without surface treatment is 0.1 mg / cm 2 .

[0093] Comparative Example 3

[0094] The difference from Example 1 is that the adhesive film is not surface treated.

[0095] Performance Testing

[0096] Peel strength test method: refer to standard GB / T29848 "Ethylene-vinyl acetate copolymer film for photovoltaic encapsulation". Conventional photovoltaic glass is selected for the peel strength between film and glass. When testing the peel strength between film and cell, the test is carried out in the stacking order of glass, conventional film, cell, test film, and conventional backplane. The first side of the encapsulation film contacts the cell, and the second side of the encapsulation film contacts the glass. Cells are selected as HJT structure cells. Before the sample test, PCT aging treatment is carried out in accordance with standard GB / T29848 "Ethylene-vinyl acetate copolymer film for photovoltaic encapsulation". The test temperature is 121°C, the test relative humidity is 100%, and the aging time is 48h.

[0097] Water vapor transmission rate test method: refer to standard GB / T29848 "Ethylene-vinyl acetate copolymer film for photovoltaic encapsulation".

[0098] Light transmittance test method: refer to standard GB / T29848 "Ethylene-vinyl acetate copolymer film for photovoltaic encapsulation".

[0099] Film hardness test method: refer to standard GB / T2411-2018 "Determination of indentation hardness (Shore hardness) of plastics and hard rubber using a hardness tester".

[0100] The encapsulation adhesive films prepared in the examples and comparative examples were tested for battery side peel strength, glass side peel strength, water vapor transmission rate, light transmittance and hardness. The test results are shown in Table 1.

[0101] Table 1

[0102]

[0103]

[0104] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:

[0105] The existing encapsulation film has insufficient encapsulation reliability for new cell modules. When the density of the surface polar groups of the encapsulation film is too low, the peel strength between the encapsulation film and the contact substrate is insufficient, especially the peel strength between the encapsulation film and the cell is insufficient, resulting in reduced reliability of the photovoltaic module in long-term use. When the density of the surface polar groups of the encapsulation film is too high, the difficulty of production and processing of the encapsulation film increases, which is not conducive to improving the production efficiency of the encapsulation film. At the same time, the adhesion between the encapsulation film and the cell is not improved more significantly. Moreover, the high density of the polar groups may cause the water vapor barrier of the photovoltaic module to decrease, which is not conducive to the long-term reliability of the photovoltaic module. The surface density of the polar groups on at least one side of the encapsulation film is controlled to be 0.5-2.5 mg / cm 2 The polar group surface density of the encapsulating film is within the range of 0.5 to 2.5 mg / cm 2 The surface on one side is arranged in contact with the battery cell, which helps to improve the intermolecular interaction force between the packaging film and the surface components of the battery cell, thereby improving the peeling strength between the packaging film and the battery cell.

[0106] The above are only embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A packaging film, characterized in that: In parts by weight, the composition of the packaging film comprises: 100 parts of base resin; 0.1 to 2 parts of a cross-linking agent; 0.1 to 5 parts of a silane coupling agent; and 0.1 to 3 parts of additives; The packaging film contains polar groups on at least one surface, and the surface density of the polar groups is 0.5 to 2.5 mg / cm 2 ; The polar group is selected from any one or more of a hydroxyl group, a carbonyl group, a carboxyl group, an epoxy group, an amide group, a silane group and an anhydride group.

2. The packaging film according to claim 1, characterized in that: The encapsulation film comprises a first surface and a second surface, wherein the surface density of polar groups on the first surface is greater than or equal to the surface density of polar groups on the second surface; preferably, the surface density of polar groups on the first surface is 0.5 to 2.5 mg / cm 2 The surface density of polar groups on the second surface is less than 0.5 mg / cm 2 .

3. The packaging film according to claim 2, characterized in that: The polar group is a silaneoxy group, and the difference between the surface density of the silaneoxy groups on the first surface and the surface density of the silaneoxy groups on the second surface is 0.5 to 2.5 mg / cm 2 .

4. The encapsulation film according to any one of claims 1 to 3, characterized in that: The peel strength between the packaging film and the battery cell is 29-53 mN / m; and / or the water vapor permeability of the packaging film is 3.1-3.5%; and / or the light transmittance of the packaging film is 89.2-90.6%; and / or the hardness of the packaging film is 55-66 HA; and / or the melt index of the matrix resin is 1.0-30 g / 10 min; and / or the light transmittance of the matrix resin is ≥88%; and / or the matrix resin is selected from any one or more of ethylene-vinyl acetate copolymer, polyolefin elastomer, polyethylene, polypropylene and ethylene propylene diene monomer rubber.

5. A method for preparing the encapsulation film according to any one of claims 1 to 4, characterized in that: The preparation method comprises: performing surface treatment on at least one surface of a film prepared from a composition of a packaging film to obtain a packaging film; the surface treatment comprises plasma treatment, spray treatment and baking treatment performed in sequence; The spray-treated solution contains a polar group source, the mass concentration of the polar group source in the spray-treated solution is 1 to 10 wt %, the spray velocity of the spray-treated solution is 0.5 to 5 L / h, and the spray treatment time is 30 to 60 s; The polar group source is selected from any one or more of a hydroxyl source, a carbonyl source, a carboxyl source, an epoxy source, an amide source, a silaneoxy source and an anhydride source.

6. The preparation method according to claim 5, characterized in that: The plasma treated gas is a nitrogen-containing gas, preferably the nitrogen-containing gas is selected from any one or more of nitrogen, ammonia, nitrous oxide and nitrogen dioxide; further preferably, the nitrogen-containing gas is nitrogen; and / or the flow rate of the nitrogen-containing gas is 5 to 50 L / min.

7. The preparation method according to claim 5 or 6, characterized in that: The hydroxyl source is hydroxyethyl methacrylate and / or hydroxyethyl acrylate; And / or, the carbonyl source is selected from any one or more of methyl methacrylate, butyl methacrylate and tert-butyl methacrylate; And / or, the carboxyl source is selected from any one or more of methacrylic acid, acrylic acid and itaconic acid; And / or, the epoxy source is glycidyl methacrylate and / or 2,3-epoxypropyl acrylate; and / or, the amide source is acrylamide and / or methacrylamide; And / or, the silaneoxy source is selected from any one or more of vinyl trimethoxy silane, vinyl triethoxy silane, γ-methacryloxypropyl trimethoxy silane coupling agent and vinyl silane; And / or, the acid anhydride source is selected from any one or more of maleic anhydride, acrylic anhydride and methacrylic anhydride; And / or, the spray treatment solution further comprises a solvent, and the solvent is selected from any one or more of n-hexane, ethanol, ethyl acetate, 1,2-dichloroethane, methanol and isopropanol.

8. The preparation method according to any one of claims 5 to 7, characterized in that: The discharge power of the plasma treatment is 500-8000W; and / or, the discharge gas pressure of the plasma treatment is 10-101325Pa; and / or, the time of the plasma treatment is 10-50s; And / or, the baking treatment temperature is 50-90° C.; and / or, the baking treatment time is 0.2-1.0 min.

9. A photovoltaic module, characterized in that: The photovoltaic module contains the encapsulation film according to any one of claims 1 to 4.

10. The photovoltaic module according to claim 9, characterized in that: The polar group surface density of the packaging film is 0.5 to 2.5 mg / cm 2 One side surface is in contact with the battery cell.