High-weather-resistance engineering joint sealing impermeable material and preparation method thereof
By adding ultrafine mica powder and nanotitanium dioxide to the engineering joint sealing materials, combined with polymer raw materials and additives, the problem of poor weather resistance of existing materials in high-altitude and cold areas is solved, and the material is realized at low temperatures and high weather resistance under high ultraviolet rays extend the service life of the building.
Patent Information
- Application Number
- CN202411409639.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-10
- Publication Date
- 2024-12-06
AI Technical Summary
The existing engineering joint sealing materials have poor weather resistance under low temperature and high ultraviolet radiation in high altitude and cold areas, resulting in building cracking, water seepage and other problems, affecting service life.
Using high weather resistance engineering seam sealing materials, by adding ultrafine mica powder and nanotitanium dioxide to the material, combining polymer raw materials and additives, a material with light reflection ability is formed to reduce the influence of ultraviolet radiation, and The use of vacuum conditions and specific temperature control during the preparation process improves the weather resistance of the material.
In the 1000-hour artificial climate aging experiment, the tensile strength and elongation rate of breaking reached more than 80%, which significantly improved the weather resistance in strong ultraviolet areas and extended the service life of the building.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of engineering caulking materials, and in particular to a highly weather-resistant engineering joint sealing and anti-seepage material and a preparation method thereof. Background Art
[0002] Engineering joint sealing materials are a kind of viscous colloid in a flowing or semi-flowing state. They are often used to fill expansion joints, settlement joints, construction joints of various materials such as concrete, asphalt concrete, reinforced concrete, wire mesh concrete, etc. in water conservancy, transportation, and municipal engineering, or to be coated on the surface of the above substrates. The engineering joint sealing materials and the substrate are firmly bonded to the substrate through van der Waals force and chemical cross-linking reaction after solidification, which can play the role of isolation, anti-seepage and anti-cracking of the substrate.
[0003] In my country's high-altitude and severely cold regions, the lowest winter temperature can reach around -55°C. At the same time, these regions have long sunshine hours and high ultraviolet radiation intensity, and temperature and ultraviolet radiation are the main factors affecting the service life and mechanical strength of engineering joint sealing materials. The weather resistance of engineering joint sealing materials in the prior art is poor. When used in these high-altitude and severely cold regions, long-term low-temperature erosion and high-intensity ultraviolet radiation will cause the engineering joint sealing materials to age, which will cause cracks and water seepage in engineering buildings, seriously affecting the service life of engineering buildings. Summary of the invention
[0004] The invention provides a highly weather-resistant engineering joint sealing and anti-seepage material and a preparation method thereof, which are used to solve the problem of poor weather resistance of the engineering joint sealing material in the prior art.
[0005] The invention provides a high-weather-resistant engineering joint sealing and anti-seepage material, which comprises a component A and a component B in a weight ratio of 1:(1-2). Component A comprises the following raw materials by weight percentage: polyether polyol, 34-36wt%. Tetrahydrofuran-propylene oxide copolymer glycol, 28-30wt%. 1,2-propylene glycol, 9-12wt%. Toluene diisocyanate, 15-18wt%. Isophorone diisocyanate, 8-12wt%. UV-327, 0.05-0.08wt%. Antioxidant 1010, 0.05-0.08wt%. Component B comprises the following raw materials by weight percentage: 1,2-propylene glycol, 20-25wt%. Nano titanium dioxide, 10-12wt%. Ultrafine muscovite powder, 10-12wt%. Light calcium carbonate, 7-14wt%. Ethylene glycol, 22-27 wt%. Diethylene glycol, 21-23 wt%. Diethylenetriamine, 3-5 wt%. 4,4'-di-tert-octyl-diphenylamine, 0.2-0.4 wt%.
[0006] Optionally, the molecular weight of the polyether polyol is 8,000, and the molecular weight of the tetrahydrofuran-propylene oxide copolymer glycol is 3,000.
[0007] Optionally, the diameter of nano titanium dioxide is 5 nanometers, and the mesh size of the ultrafine muscovite powder is 5000 meshes.
[0008] Optionally, the mass ratio of UV-327 to antioxidant 1010 is 1:1.
[0009] Optionally, the mass ratio of nano titanium dioxide to ultrafine muscovite powder is 1:1.
[0010] The present invention also provides a method for preparing a highly weather-resistant engineering joint sealing and anti-seepage material, the method for preparing a highly weather-resistant engineering joint sealing and anti-seepage material comprising: preparing component A, preparing component B, and mixing components A and B.
[0011] Optionally, the preparation process of component A includes the following steps:
[0012] The following raw materials are weighed by weight percentage: polyether polyol, 34-36wt%. Tetrahydrofuran-propylene oxide copolymer glycol, 28-30wt%. 1,2-propylene glycol, 9-12wt%. Toluene diisocyanate, 15-18wt%. Isophorone diisocyanate, 8-12wt%. UV-327, 0.05-0.08wt%. Antioxidant 1010, 0.05-0.08wt%.
[0013] Add polyether polyol, tetrahydrofuran-propylene oxide copolymer and 1,2-propylene glycol into the reaction kettle, turn on the stirrer, and heat to 55-65°C.
[0014] Start the vacuum pump and raise the vacuum degree to 0.095-0.1MPa.
[0015] Continue to raise the temperature to 110-120°C and maintain for 3.5-4.5 hours.
[0016] The temperature was lowered to 75-85°C, toluene diisocyanate and isophorone diisocyanate were added dropwise simultaneously, and the mixture was stirred and reacted under vacuum for 5 hours.
[0017] The temperature was lowered to 35-45°C, UV-327 and antioxidant 1010 were added, and stirring was continued under vacuum for 15-25 minutes to obtain component A.
[0018] Optionally, the preparation process of component B includes the following steps:
[0019] The following raw materials are weighed in weight percentage: 1,2-propylene glycol, 20-25wt%. Nano titanium dioxide, 10-12wt%. Ultrafine muscovite powder, 10-12wt%. Light calcium carbonate, 7-14wt%. Ethylene glycol, 22-27wt%. Diethylene glycol, 21-23wt%. Diethylenetriamine, 3-5wt%. 4,4'-di-tert-octyl-diphenylamine, 0.2-0.4wt%.
[0020] Place nano titanium dioxide, ultrafine muscovite powder and light calcium carbonate in an oven at 120°C and dry for 8 hours.
[0021] Add 1,2-propylene glycol, ethylene glycol, diethylene glycol, dried nano titanium dioxide, ultrafine muscovite powder, and light calcium carbonate into the reactor, start the vacuum pump to raise the vacuum degree to 0.095-0.1MPa, and at the same time raise the temperature to 120-125°C and maintain for 2h.
[0022] The temperature was lowered to 45-55°C, diethylenetriamine and 4,4'-di-tert-octyl-diphenylamine were added, and the mixture was stirred under vacuum for 1 hour to obtain component B.
[0023] Optionally, the mixture of components A and B, that is, mixing component A and component B at a mass ratio of 1:(1-2) and stirring them evenly, can obtain a highly weather-resistant engineering joint sealing and anti-seepage material.
[0024] Optionally, after preparation, component A and component B are placed in a sealed container under nitrogen protection for standby use.
[0025] The high weather resistance engineering joint sealing and anti-seepage material provided by the present invention has the beneficial effect that: by combining ultrafine white mica, ultrafine nano titanium dioxide with polymer raw materials and additives, the weather resistance of the engineering joint sealing material in areas with strong ultraviolet radiation can be improved, and after artificial climate aging test (1000h), the tensile strength retention rate and the elongation at break retention rate can still reach more than 80%. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention is clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work also fall within the scope of protection of the present invention.
[0027] The invention provides a high-weather-resistant engineering joint sealing and anti-seepage material, which comprises a component A and a component B in a weight ratio of 1:(1-2). Component A comprises the following raw materials by weight percentage: polyether polyol, 34-36wt%. Tetrahydrofuran-propylene oxide copolymer glycol, 28-30wt%. 1,2-propylene glycol, 9-12wt%. Toluene diisocyanate, 15-18wt%. Isophorone diisocyanate, 8-12wt%. UV-327, 0.05-0.08wt%. Antioxidant 1010, 0.05-0.08wt%. Component B comprises the following raw materials by weight percentage: 1,2-propylene glycol, 20-25wt%. Nano titanium dioxide, 10-12wt%. Ultrafine muscovite powder, 10-12wt%. Light calcium carbonate, 7-14wt%. Ethylene glycol, 22-27 wt%. Diethylene glycol, 21-23 wt%. Diethylenetriamine, 3-5 wt%. 4,4'-di-tert-octyl-diphenylamine, 0.2-0.4 wt%.
[0028] Highly weather-resistant engineering joint sealing and anti-seepage materials have two main uses: one is to fill in gaps such as expansion joints and settlement joints in engineering buildings. When the highly weather-resistant engineering joint sealing and anti-seepage materials are cured, the seam wall, seam bottom and highly weather-resistant engineering joint sealing and anti-seepage materials will bond into an integral structure. Since the highly weather-resistant engineering joint sealing and anti-seepage materials themselves have great elasticity, they can eliminate the stress generated by temperature in the structure through their own deformation, thereby ensuring the stability of the engineering structure. At the same time, they can also play the role of connection, anti-seepage and adaptation to dynamic load deformation. The second is to coat the highly weather-resistant engineering joint sealing and anti-seepage materials on the surface of the substrate, and after curing, they will bond with the substrate as a whole, which plays the role of isolation from the external environment, anti-seepage, waterproofing and anti-cracking.
[0029] The high weather-resistant engineering joint sealing and anti-seepage material provided by the present invention has ultrafine muscovite powder and nano titanium dioxide added to the raw materials, and the ultrafine muscovite powder and nano titanium dioxide are mixed with the polymer material and other additives in the raw materials to obtain the high weather-resistant engineering joint sealing and anti-seepage material with light reflection ability.
[0030] Among them, the ultrafine muscovite powder is a flat reflective reflector, and the nano titanium dioxide is a rutile type and anatase type spinel. Both of them can emit the absorbed sunlight and heat into the air at a certain wavelength, and can reflect the spectral energy of sunlight at 400-1800nm. The above two substances are compounded in a certain proportion and synthesized with other polymer raw materials and additives to obtain a highly weather-resistant engineering joint sealing and anti-seepage material that can reflect ultraviolet rays, thereby reducing the impact of ultraviolet radiation on the material. At the same time, ultraviolet absorber UV-237 and antioxidant 1010 are added to the material. These two synergistically improve the low temperature performance and ultraviolet resistance of the highly weather-resistant engineering joint sealing and anti-seepage material with other raw materials.
[0031] Furthermore, the molecular weight of the polyether polyol is 8000, and the molecular weight of the tetrahydrofuran-propylene oxide copolymer glycol is 3000.
[0032] Furthermore, the diameter of the nano titanium dioxide is 5 nanometers, and the mesh size of the ultrafine muscovite powder is 5000 meshes.
[0033] Furthermore, the mass ratio of UV-327 to antioxidant 1010 is 1:1.
[0034] Furthermore, the mass ratio of nano titanium dioxide to ultrafine muscovite powder is 1:1.
[0035] Furthermore, the preparation method of the highly weather-resistant engineering joint sealing and anti-seepage material includes: preparing component A, preparing component B, and mixing components A and B.
[0036] Furthermore, the preparation process of component A includes the following steps:
[0037] The following raw materials are weighed by weight percentage: polyether polyol, 34-36wt%. Tetrahydrofuran-propylene oxide copolymer glycol, 28-30wt%. 1,2-propylene glycol, 9-12wt%. Toluene diisocyanate, 15-18wt%. Isophorone diisocyanate, 8-12wt%. UV-327, 0.05-0.08wt%. Antioxidant 1010, 0.05-0.08wt%.
[0038] Add polyether polyol, tetrahydrofuran-propylene oxide copolymer and 1,2-propylene glycol into the reaction kettle, turn on the stirrer, and heat to 55-65°C.
[0039] Start the vacuum pump and raise the vacuum degree to 0.095-0.1MPa.
[0040] Continue to raise the temperature to 110-120°C and maintain for 3.5-4.5 hours.
[0041] The temperature was lowered to 75-85°C, toluene diisocyanate and isophorone diisocyanate were added dropwise simultaneously, and the mixture was stirred and reacted under vacuum for 5 hours.
[0042] The temperature was lowered to 35-45°C, UV-327 and antioxidant 1010 were added, and stirring was continued under vacuum for 15-25 minutes to obtain component A.
[0043] Furthermore, the preparation process of component B includes the following steps:
[0044] The following raw materials are weighed in weight percentage: 1,2-propylene glycol, 20-25wt%. Nano titanium dioxide, 10-12wt%. Ultrafine muscovite powder, 10-12wt%. Light calcium carbonate, 7-14wt%. Ethylene glycol, 22-27wt%. Diethylene glycol, 21-23wt%. Diethylenetriamine, 3-5wt%. 4,4'-di-tert-octyl-diphenylamine, 0.2-0.4wt%.
[0045] Place nano titanium dioxide, ultrafine muscovite powder and light calcium carbonate in an oven at 120°C and dry for 8 hours.
[0046] Add 1,2-propylene glycol, ethylene glycol, diethylene glycol, dried nano titanium dioxide, ultrafine muscovite powder, and light calcium carbonate into the reactor, start the vacuum pump to raise the vacuum degree to 0.095-0.1MPa, and at the same time raise the temperature to 120-125°C and maintain for 2h.
[0047] The temperature was lowered to 45-55°C, diethylenetriamine and 4,4'-di-tert-octyl-diphenylamine were added, and the mixture was stirred under vacuum for 1 hour to obtain component B.
[0048] Furthermore, the mixture of component A and component B, i.e., mixing component A and component B at a mass ratio of 1:(1-2) and stirring evenly, can obtain a highly weather-resistant engineering joint sealing and anti-seepage material. The prepared highly weather-resistant engineering joint sealing and anti-seepage material can be filled in the joint or coated on the surface of the substrate, thereby achieving the effects of sealing, anti-seepage, adaptability to deformation, isolation and waterproofing.
[0049] Furthermore, after the preparation of component A and component B is completed, they are placed in a sealed container under nitrogen protection for standby use.
[0050] The highly weather-resistant engineering joint sealing and anti-seepage material provided by the present invention can achieve the technical indicators shown in Table 1:
[0051] Table 1
[0052]
[0053] The present invention is further described in detail below in conjunction with specific embodiments.
[0054] Example 1
[0055] A highly weather-resistant engineering joint sealing and anti-seepage material comprises a component A of the following weight percentage components: 34wt% polyether polyol (molecular weight 8000), 28wt% tetrahydrofuran-propylene oxide copolymer glycol (molecular weight 3000), 9wt% 1,2-propylene glycol, 16.84wt% toluene diisocyanate, 12wt% isophorone diisocyanate, 0.08wt% UV-327, and 0.08wt% antioxidant 1010.
[0056] The second component also includes the following weight percentage components: 1,2-propylene glycol, 20wt%. Nano titanium dioxide (5nm), 12wt%. Ultrafine muscovite powder (5000 mesh), 12wt%. Light calcium carbonate, 7.8wt%. Ethylene glycol, 22wt%. Diethylene glycol, 21wt%. Diethylenetriamine, 5wt%. 4,4'-di-tert-octyl-diphenylamine, 0.2wt%.
[0057] A method for preparing a highly weather-resistant engineering joint sealing and anti-seepage material comprises the following steps:
[0058] 1) Preparation of component A: After weighing, add polyether polyol, tetrahydrofuran-propylene oxide copolymer and 1,2-propylene glycol into a reaction kettle, turn on the stirrer, and heat to 55°C.
[0059] Start the vacuum pump and raise the vacuum degree to 0.095MPa.
[0060] Continue to raise the temperature to 110°C and maintain for 3.5 hours.
[0061] The temperature was lowered to 75°C, toluene diisocyanate and isophorone diisocyanate were added dropwise simultaneously, and the mixture was stirred and reacted under vacuum for 5 hours.
[0062] The temperature was lowered to 35°C, UV-327 and antioxidant 1010 were added, and stirring was continued under vacuum for 15 minutes to obtain component A.
[0063] 2) Preparation of component B: After weighing, place nano titanium dioxide, ultrafine muscovite powder and light calcium carbonate in an oven at 120° C. and dry for 8 hours.
[0064] Add 1,2-propylene glycol, ethylene glycol, diethylene glycol, dried nano titanium dioxide, ultrafine muscovite powder, and light calcium carbonate into the reactor, start the vacuum pump to raise the vacuum degree to 0.095 MPa, and at the same time raise the temperature to 120°C and maintain for 2 hours.
[0065] The temperature was lowered to 45°C, diethylenetriamine and 4,4'-di-tert-octyl-diphenylamine were added, and the mixture was stirred under vacuum for 1 hour to obtain component B.
[0066] 3) Mixing of components A and B: Mix the prepared components A and B in a ratio of 1:2 and stir evenly to obtain a highly weather-resistant engineering joint sealing and anti-seepage material. The prepared highly weather-resistant engineering joint sealing and anti-seepage material can be filled in the joint or coated on the surface of the substrate.
[0067] The technical indicators of the high weather resistance engineering joint sealing and anti-seepage material of this embodiment are shown in Table 2:
[0068] Table 2
[0069]
[0070]
[0071] Example 2
[0072] A highly weather-resistant engineering joint sealing and anti-seepage material comprises a component A of the following weight percentage components: 35wt% polyether polyol (molecular weight 8000), 28wt% tetrahydrofuran-propylene oxide copolymer glycol (molecular weight 3000), 9.88wt% 1,2-propylene glycol, 17wt% toluene diisocyanate, 10wt% isophorone diisocyanate, 0.06wt% UV-327, and 0.06wt% antioxidant 1010.
[0073] The second component also includes the following weight percentage components: 1,2-propylene glycol, 20wt%. Nano titanium dioxide (5nm), 11wt%. Ultrafine muscovite powder (5000 mesh), 11wt%. Light calcium carbonate, 10.7wt%. Ethylene glycol, 22wt%. Diethylene glycol, 21wt%. Diethylenetriamine, 4wt%. 4,4'-di-tert-octyl-diphenylamine, 0.3wt%.
[0074] A method for preparing a highly weather-resistant engineering joint sealing and anti-seepage material comprises the following steps:
[0075] 1) Preparation of component A: After weighing, add polyether polyol, tetrahydrofuran-propylene oxide copolymer and 1,2-propylene glycol into a reaction kettle, turn on the stirrer, and heat to 65°C.
[0076] Start the vacuum pump and raise the vacuum degree to 0.1MPa.
[0077] Continue to raise the temperature to 120°C and maintain for 4.5 hours.
[0078] The temperature was lowered to 85°C, toluene diisocyanate and isophorone diisocyanate were added dropwise simultaneously, and the mixture was stirred and reacted for 5 hours under vacuum.
[0079] The temperature was lowered to 45°C, UV-327 and antioxidant 1010 were added, and stirring was continued under vacuum for 25 minutes to obtain component A.
[0080] 2) Preparation of component B: After weighing, place nano titanium dioxide, ultrafine muscovite powder and light calcium carbonate in an oven at 120° C. and dry for 8 hours.
[0081] Add 1,2-propylene glycol, ethylene glycol, diethylene glycol, dried nano titanium dioxide, ultrafine muscovite powder, and light calcium carbonate into the reactor, start the vacuum pump to raise the vacuum degree to 0.1 MPa, and at the same time raise the temperature to 125°C and maintain for 2 hours.
[0082] The temperature was lowered to 55° C., diethylenetriamine and 4,4'-di-tert-octyl-diphenylamine were added, and the mixture was stirred under vacuum for 1 hour to obtain component B.
[0083] 3) Mixing of components A and B: Mix the prepared components A and B in a ratio of 1:1.5 and stir evenly to obtain a highly weather-resistant engineering joint sealing and anti-seepage material. The prepared highly weather-resistant engineering joint sealing and anti-seepage material can be filled in the joint or coated on the surface of the substrate.
[0084] The technical indicators of the high weather resistance engineering joint sealing and anti-seepage material of this embodiment are shown in Table 3:
[0085] Table 3
[0086]
[0087] Example 3
[0088] A highly weather-resistant engineering joint sealing and anti-seepage material comprises a component A of the following weight percentage components: 35wt% polyether polyol (molecular weight 8000), 29.4wt% tetrahydrofuran-propylene oxide copolymer glycol (molecular weight 3000), 10wt% 1,2-propylene glycol, 15.2wt% toluene diisocyanate, 10.3wt% isophorone diisocyanate, 0.05wt% UV-327, and 0.05wt% antioxidant 1010.
[0089] The second component also includes the following weight percentage components: 1,2-propylene glycol, 22wt%. Nano titanium dioxide (5nm), 9wt%. Ultrafine muscovite powder (5000 mesh), 9wt%. Light calcium carbonate, 8.6wt%. Ethylene glycol, 26wt%. Diethylene glycol, 22wt%. Diethylenetriamine, 3wt%. 4,4'-di-tert-octyl-diphenylamine, 0.4wt%.
[0090] A method for preparing a highly weather-resistant engineering joint sealing and anti-seepage material comprises the following steps:
[0091] 1) Preparation of component A: After weighing, add polyether polyol, tetrahydrofuran-propylene oxide copolymer and 1,2-propylene glycol into a reaction kettle, turn on the stirrer, and heat to 60°C.
[0092] Start the vacuum pump and raise the vacuum degree to 0.095MPa.
[0093] Continue to raise the temperature to 115°C and maintain for 4 hours.
[0094] The temperature was lowered to 80°C, toluene diisocyanate and isophorone diisocyanate were added dropwise simultaneously, and the mixture was stirred and reacted under vacuum for 5 hours.
[0095] The temperature was lowered to 40°C, UV-327 and antioxidant 1010 were added, and stirring was continued under vacuum for 20 minutes to obtain component A.
[0096] 2) Preparation of component B: After weighing, place nano titanium dioxide, ultrafine muscovite powder and light calcium carbonate in an oven at 120° C. and dry for 8 hours.
[0097] Add 1,2-propylene glycol, ethylene glycol, diethylene glycol, dried nano titanium dioxide, ultrafine muscovite powder, and light calcium carbonate into the reactor, start the vacuum pump to raise the vacuum degree to 0.095 MPa, and at the same time raise the temperature to 120°C and maintain for 2 hours.
[0098] The temperature was lowered to 50°C, diethylenetriamine and 4,4'-di-tert-octyl-diphenylamine were added, and the mixture was stirred under vacuum for 1 hour to obtain component B.
[0099] 3) Mixing of components A and B: Mix the prepared components A and B in a ratio of 1:1 and stir evenly to obtain a highly weather-resistant engineering joint sealing and anti-seepage material. The prepared highly weather-resistant engineering joint sealing and anti-seepage material can be filled in the joint or coated on the surface of the substrate.
[0100] The technical indicators of the high weather resistance engineering joint sealing and anti-seepage material of this embodiment are shown in Table 4:
[0101] Table 4
[0102]
[0103]
[0104] Comparative Example 1
[0105] The difference between Comparative Example 1 and Example 3 is that nano titanium dioxide and ultrafine muscovite powder are not added to component B, and the weight percentages of the other components are: 1,2-propylene glycol, 22wt%. Light calcium carbonate, 26.6wt%. Ethylene glycol, 26wt%. Diethylene glycol, 22wt%. Diethylenetriamine, 3wt%. 4,4'-di-tert-octyl-diphenylamine, 0.4wt%.
[0106] The technical indicators of the high weather resistance engineering joint sealing and anti-seepage material of Comparative Example 1 are shown in Table 5:
[0107] Table 5
[0108]
[0109]
[0110] It can be seen from the data of Comparative Example 1 and Example 3 that under the condition of adding light-reflecting materials (nano titanium dioxide and ultra-white fine mica powder), the artificial weathering aging performance of the high-weather-resistant engineering joint sealing and anti-seepage material is greatly improved compared to the artificial weathering aging performance of the material without adding light-reflecting materials. This is because nano titanium dioxide is a rutile anatase spinel, and ultra-fine white mica powder is a flat reflective reflector. Both substances can emit the absorbed sunlight and heat into the air at a certain wavelength, and can reflect the spectral energy of sunlight at 400-1800nm. Nano titanium dioxide and ultra-white fine mica powder are compounded, and matched with other polymer raw materials and additives in component A and component B. The finally obtained high-weather-resistant engineering joint sealing and anti-seepage material can reflect ultraviolet rays and reduce the temperature of the material itself, thereby reducing the impact of ultraviolet radiation on the material and enhancing the material's ability to resist ultraviolet rays.
[0111] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features therein may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A highly weather-resistant engineering joint sealing and anti-seepage material, It is characterized in that The highly weather-resistant engineering joint sealing and anti-seepage material comprises a component A and a component B in a weight ratio of 1:(1-2); The component A comprises the following raw materials by weight percentage: polyether polyol, 34-36wt%; tetrahydrofuran-propylene oxide copolymer glycol, 28-30wt%; 1,2-propylene glycol, 9-12wt%; toluene diisocyanate, 15-18wt%; isophorone diisocyanate, 8-12wt%; UV-327, 0.05-0.08wt%; antioxidant 1010, 0.05-0.08wt%; The component B comprises the following raw materials in terms of weight percentage: 1,2-propylene glycol, 20-25wt%; nano titanium dioxide, 10-12wt%; ultrafine muscovite powder, 10-12wt%; light calcium carbonate, 7-14wt%; ethylene glycol, 22-27wt%; diethylene glycol, 21-23wt%; diethylenetriamine, 3-5wt%; and 4,4'-di-tert-octyl-diphenylamine, 0.2-0.4wt%.
2. The highly weather-resistant engineering joint sealing and anti-seepage material according to claim 1, It is characterized in that The molecular weight of the polyether polyol is 8000, and the molecular weight of the tetrahydrofuran-propylene oxide copolymer glycol is 3000.
3. The highly weather-resistant engineering joint sealing and anti-seepage material according to claim 1, It is characterized in that The diameter of the nano titanium dioxide is 5 nanometers, and the mesh number of the ultrafine muscovite powder is 5000 meshes.
4. The highly weather-resistant engineering joint sealing and anti-seepage material according to claim 1, It is characterized in that The mass ratio of the UV-327 to the antioxidant 1010 is 1:
1.
5. The highly weather-resistant engineering joint sealing and anti-seepage material according to claim 1, It is characterized in that The mass ratio of the nano titanium dioxide to the ultrafine muscovite powder is 1:
1.
6. A method for preparing the highly weather-resistant engineering joint sealing and anti-seepage material according to any one of claims 1 to 5, It is characterized in that The preparation method of the highly weather-resistant engineering joint sealing and anti-seepage material comprises: Preparation of component A; Preparation of component B; Mixing of components A and B.
7. The method for preparing the highly weather-resistant engineering joint sealing and anti-seepage material according to claim 6, It is characterized in that The production process of the component A comprises the following steps: The following raw materials are weighed by weight percentage: polyether polyol, 34-36wt%; tetrahydrofuran-propylene oxide copolymer glycol, 28-30wt%; 1,2-propylene glycol, 9-12wt%; toluene diisocyanate, 15-18wt%; isophorone diisocyanate, 8-12wt%; UV-327, 0.05-0.08wt%; antioxidant 1010, 0.05-0.08wt%; Add polyether polyol, tetrahydrofuran-propylene oxide copolymer glycol and 1,2-propylene glycol into the reaction kettle, turn on the stirrer, and heat to 55-65°C; Start the vacuum pump to raise the vacuum degree to 0.095-0.1MPa; Continue to raise the temperature to 110-120°C and maintain for 3.5-4.5 hours; Cool down to 75-85°C, add toluene diisocyanate and isophorone diisocyanate dropwise simultaneously, and stir to react for 5 hours under vacuum; The temperature was lowered to 35-45° C., UV-327 and antioxidant 1010 were added, and the mixture was stirred under vacuum for 15-25 minutes to obtain the component A.
8. The method for preparing the highly weather-resistant engineering joint sealing and anti-seepage material according to claim 6, It is characterized in that The preparation process of the component B comprises the following steps: The following raw materials are weighed according to weight percentage: 1,2-propylene glycol, 20-25wt%; nano titanium dioxide, 10-12wt%; ultrafine muscovite powder, 10-12wt%; light calcium carbonate, 7-14wt%; ethylene glycol, 22-27wt%; diethylene glycol, 21-23wt%; diethylenetriamine, 3-5wt%; 4,4'-di-tert-octyl-diphenylamine, 0.2-0.4wt%; Place nano titanium dioxide, ultrafine muscovite powder and light calcium carbonate in an oven at 120°C and dry for 8 hours; Add 1,2-propylene glycol, ethylene glycol, diethylene glycol, dried nano titanium dioxide, ultrafine muscovite powder, and light calcium carbonate into the reactor, start the vacuum pump to raise the vacuum degree to 0.095-0.1MPa, and raise the temperature to 120-125°C for 2h; The temperature was lowered to 45-55° C., diethylenetriamine and 4,4'-di-tert-octyl-diphenylamine were added, and the mixture was stirred under vacuum for 1 hour to obtain the component B.
9. The method for preparing the highly weather-resistant engineering joint sealing and anti-seepage material according to claim 6, It is characterized in that The mixing of the two components A and B is to mix the component A and the component B at a mass ratio of 1: (1-2) and stir them evenly to obtain the high weather resistance engineering joint sealing and anti-seepage material.
10. The method for preparing the highly weather-resistant engineering joint sealing and anti-seepage material according to claim 6, It is characterized in that After the preparation of the component A and the component B is completed, they are placed in a sealed container under nitrogen protection for standby use.