Reversible photochromic material as well as preparation method and application thereof

Through the interlaced laminated structure and cyano group modification of Na-C3N5 nanosheets, the problem of poor stability of carbon nitride photochromic materials under aerobic conditions is solved, and the reversible photochromic and high stability in an aerobic environment is achieved , suitable for the application of decorative and information storage materials.

CN119081674APending Publication Date: 2024-12-06JIANGSU UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411190293.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing carbon nitride photochromic materials have poor stability under aerobic conditions and do not last long, which limits their wide application in practical applications.

Method used

Using the interlaced laminated structure of Na-C3N5 nanosheets, sodium chloride, sodium hydroxide and 3-amino-1,2,4-triazole as precursors are synthesized by one-step calcination method to form high crystallinity and growth in specific directions. Nanosheets, cyano groups are introduced to enhance charge storage function and improve the chemical and thermal stability of the material through the synergistic action of NaCl and NaOH.

Benefits of technology

Materials that are reversible photochromic under aerobic conditions have faster discoloration efficiency, fuller discoloration depth and highly reversible color changes, while improving the chemical and thermal stability of the material, suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081674A_ABST
    Figure CN119081674A_ABST
Patent Text Reader

Abstract

The invention discloses a reversible photochromic material as well as a preparation method and application thereof. The photochromic material is formed by stacking Na-C3N5 nanosheets in a staggered mode, and the Na-C3N5 nanosheets are obtained by polymerizing sodium chloride, sodium hydroxide and a precursor. The reversible photochromic material is prepared by an alkaline sodium salt assisted molten salt one-step method, the operation is convenient and fast, the reversible photochromic material is suitable for large-scale production, the prepared reversible photochromic material breaks through the limit that a common carbon nitride-based material can only switch colors under an anaerobic condition, and the reversible photochromic material has higher color changing efficiency and more full color changing depth, is highly reversible in color, and is suitable for large-scale production. Meanwhile, the photochromic material also has better chemical and thermal stability, can resist corrosion and thermal decomposition in a color change process, still shows good stability after multiple times of cyclic color change, and has a wide prospect in the field of photochromism.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a reversible photochromic material, and also to a preparation method and application of the reversible photochromic material. Background Art

[0002] Photochromic materials have attracted extensive research interest in recent years and have attracted widespread attention in the fields of chemistry and biology for decades, however, such reversible color switches usually require highly uniform nanostructures of precious metals or other materials, which hinders their reuse and large-scale synthesis. Therefore, photochromic materials have potential room for improvement in stability, tunability and cost.

[0003] Carbon nitride is a compound composed of carbon and nitrogen elements, and its structure can be regulated by adjusting the carbon-nitrogen ratio, heteroatom doping, and crystal structure. These regulatory methods give carbon nitride materials unique optical and electronic properties, making them photochromic. When carbon nitride materials are exposed to light, light energy excites electrons in the material, resulting in charge transfer or adjustment of the band structure, thereby changing the optical absorption characteristics and color of the material. Existing carbon nitride color-changing materials can be mainly divided into several types, each of which has unique characteristics and limitations in its color-changing mechanism and application. First, pure carbon nitride materials are the most basic type. They achieve color change through the excitation of ultraviolet or visible light, relying on the transition of their electronic structure and the generation of photogenerated carriers. However, the color-changing effect of pure carbon nitride is usually weak, and the color will quickly return to its original state when the light stops or oxygen is present. The range of color change is mainly concentrated in the ultraviolet to blue light region, which limits its practicality in a wide range of applications.

[0004] Secondly, oxidized carbon nitride materials adjust their electronic structure and light absorption characteristics by introducing oxide groups (such as C=O or -OH) into the carbon nitride structure. Although this oxidative modification can enhance the photochromic effect of the material, the color change effect will be significantly weakened in the presence of oxygen. Although the oxide group can enhance the light absorption ability of the material, it is also more likely to react with oxygen, thereby inhibiting the photochromic effect. In addition, doped carbon nitride materials are doped by introducing other elements (such as nitrogen, sulfur, phosphorus or metal ions) to change the band structure of carbon nitride and improve its photochromic efficiency. Doping can broaden the light absorption range of the material to a certain extent, making the color change effect more obvious. However, the stability of this type of material in the air is still poor and is easily affected by oxygen, resulting in a short-lasting color change effect.

[0005] Composite carbon nitride materials form heterostructures by combining carbon nitride with other materials (such as metal oxides, precious metal nanoparticles or conductive polymers) to enhance their photochromic properties. The synergistic effect of the composite structure can usually achieve a more significant color change effect and a wider color change range. However, the preparation process of the composite material is relatively complicated and costly, and its long-term stability still needs further research and verification. Finally, structurally modified carbon nitride materials improve their photochromic properties by nanostructuring or pore modification. For example, synthetic nanosheets, nanotubes or porous structures can increase the light absorption area of ​​the material and improve the carrier separation efficiency, thereby enhancing the color change effect. Although this structural modification can increase the color change rate and effect of the material, in the air, especially in the presence of oxygen, such materials are still prone to rapid fading, and the retention time after color change is short. Although they show good photochromic effects in hypoxic or vacuum environments, their color change performance and stability are still facing challenges in practical application environments, especially in the presence of oxygen. Therefore, further research and exploration are still needed to break through the anaerobic limitation and achieve reversible photochromism under aerobic conditions. Summary of the invention

[0006] Purpose of the invention: The purpose of the present invention is to provide a reversible photochromic material that breaks through the limitation of oxygen-free conditions, and also to provide a preparation method of the above-mentioned reversible photochromic material and its application in the field of photochromism under aerobic conditions.

[0007] Technical solution: The reversible photochromic material of the present invention is composed of staggered layers of Na-C3N5 nanosheets, wherein the Na-C3N5 nanosheets are obtained by polymerization of sodium chloride and sodium hydroxide with a precursor, wherein the precursor is 3-amino-1, 2, 4-triazole.

[0008] Wherein, the mass ratio of the sodium chloride, sodium hydroxide and the precursor is 1:0.02-0.05:0.5-0.8.

[0009] Wherein, the thickness of the Na-C3N5 nanosheet is 4-6nm.

[0010] The method for preparing the above-mentioned reversible photochromic material comprises the following steps:

[0011] (1) mixing sodium chloride, sodium hydroxide and a precursor and grinding them thoroughly to obtain a mixed powder;

[0012] (2) calcining the mixed powder, and cooling to room temperature to obtain a solid material after the reaction is completed;

[0013] (3) Washing the solid material with water, centrifuging, washing and drying the solid, and grinding to obtain a medium to reversible photochromic material.

[0014] Wherein, in step (2), the calcination treatment has a temperature of 550-600°C, a heating rate of 4-6°C / min, and a holding time of 2.5-4.5h.

[0015] Wherein, in step (3), the water washing adopts deionized water, and the water washing temperature is 80-90°C.

[0016] Wherein, in step (3), after the solid material is washed with water, the chloride ion content is detected by silver nitrate detection to detect whether the chloride ions are washed clean.

[0017] Wherein, the concentration of the silver nitrate solution is 0.01M-0.1M.

[0018] The above-mentioned reversible photochromic material can also be used in the field of photochromism under aerobic conditions.

[0019] The photochromic field includes decorative materials or information storage materials, such as laminated glass.

[0020] Principle of the invention: The reversible photochromic material of the present invention is synthesized by a one-step calcination method, using the lattice structure of NaCl as a template to promote the growth of carbon nitride in a specific direction, thereby forming a sheet structure. The staggered and stacked structure of the nanosheets causes the light path to refract, which is conducive to the absorption and utilization of light, and converts the photon energy into electrons and holes more efficiently, thereby enhancing the efficiency of storing electrons, thereby achieving faster color change efficiency and more saturated color change depth. And the high crystallization method allows the material to grow in a specific direction, forming a fixed structure, which is not messy, and therefore has better chemical and thermal stability. At the same time, under high temperature conditions, the presence of NaOH helps the peeling and dispersion of carbon nitride nanosheets, preventing them from agglomerating during the growth process and increasing the surface area; secondly, during the heat treatment process, the alkaline sodium salt will decompose and release cyanide ions. During the heat treatment process, the cyanide ions will react with the carbon nitride precursor, introduce cyanide into the carbon nitride structure, and increase the charge storage function of the material by polymerizing cyanide; finally, a cyanide group-modified Na-C3N5 reversible photochromic material is obtained. By introducing cyano groups during heat treatment of alkaline sodium salts, cyano groups can be oxidized by photogenerated holes to form highly active enamide triazine radial cations, leaving photogenerated electrons stored in the material. At the same time, the interaction between sodium ions and cyano groups promotes the storage of more photogenerated electrons, extending the absorption wavelength of the material to 600nm, accompanied by a change in color from yellow to dark. This photochromic phenomenon is not only an intuitive manifestation of the electron storage process, but also the result of significant changes in the internal structure and energy band of the material.

[0021] The Na-C3N5 reversible photochromic material of the present invention has a large surface area. In the co-pyrolysis process, the synergistic effect of NaCl and NaOH promotes the reconstruction of the carbon nitride structure. As a template, NaCl can induce the delamination of the carbon nitride material at high temperature, and NaOH further weakens the interlayer van der Waals force through chemical reaction with carbon nitride, promoting the peeling of the nanosheet. The layered nanosheets finally formed not only have a larger specific surface area. The Na-C3N5 reversible photochromic material of the present invention introduces NaCl and NaOH in the co-pyrolysis process, which promotes the passivation of defect sites on the surface of the material, reduces the surface free energy, and reduces the possibility of the material reacting with external chemical substances (such as oxygen, acidic or alkaline solutions). This surface passivation significantly improves the chemical and thermal stability of the material, can resist corrosion and thermal decomposition in the color change process, which makes Na-C3N5 still show good stability after multiple cycles of color change. The color of the Na-C3N5 reversible photochromic nanosheet of the present invention is highly reversible. Compared with the previous color display principle, the metastable charge and discharge of photoelectrons does not bring about any permanent molecular or geometric structure transformation, which makes the color switch highly reversible.

[0022] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: (1) The reversible photochromic material of the present invention has a faster color change efficiency and a richer color change depth, and the color is highly reversible. The metastable charge and discharge of photoelectrons will not bring about any permanent molecular or geometric structure changes; (2) The reversible photochromic material of the present invention has better chemical and thermal stability, and can resist corrosion and thermal decomposition during the color change process, so that Na-C3N5 still shows good stability after multiple cycles of color change; (3) The one-step calcination method is easy to operate and suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 is a transmission electron microscope (TEM) image of the reversible photochromic material of the present invention;

[0024] Figure 2 X-ray diffraction (XRD) patterns of the reversible photochromic material of the present invention and comparative example C3N5;

[0025] Figure 3 The solid state of the reversible photochromic material of the present invention and the comparative example C3N5 13 C nuclear magnetic resonance (NMR) characterization;

[0026] Figure 4 It is the Fourier infrared test (FT-IR) spectrum of the reversible photochromic material of the present invention and the comparative example C3N5;

[0027] Figure 5The XPS test spectra of the reversible photochromic material of the present invention and the comparative example C3N5;

[0028] Figure 6 The UV-visible absorption spectra of the comparative example C3N5 suspension (a) and the reversible photochromic material (b) of the present invention at different irradiation times;

[0029] Figure 7 A digital photo of the reversible photochromic material of the present invention during color change and restoration;

[0030] Figure 8 The time required for complete color change and recovery of the materials of the examples and comparative examples is compared;

[0031] Fig. 9 It is the A / A0 irradiation diagram of Na-C3N5 of the reversible photochromic material of the present invention under the optical switching condition;

[0032] Fig.10 The unpaired electrons recorded by the reversible photochromic material of the present invention under dark / irradiated conditions through ESR;

[0033] Fig.11 A cyclic experiment of photochromic response on the reversible photochromic material of the present invention;

[0034] Fig.12 The X-ray diffraction (XRD) patterns of the reversible photochromic material of the present invention before and after color change. DETAILED DESCRIPTION

[0035] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.

[0036] Example 1

[0037] The reversible photochromic material Na-C3N5 of the present invention has a preparation method comprising the following steps:

[0038] (1) Sodium chloride, sodium hydroxide and 3-amino-1,2,4-triazole were ground in a mortar in a ratio of 1:0.03:0.6;

[0039] (2) The mixed powder was transferred into a 50 ml crucible and placed in a muffle furnace for calcination at 600 °C, a heating rate of 6 °C / min, and a holding time of 4 h. After the holding time was up, the mixture was cooled to room temperature.

[0040] (3) Wash the obtained brown solid with a large amount of deionized water at a temperature of 80°C; use silver nitrate to detect whether the chloride ions in the obtained brown solid aqueous solution are washed out, collect the obtained samples, centrifuge, wash, dry, and grind to obtain nanosheets labeled as Na-C3N5-6.

[0041] Example 2

[0042] The reversible photochromic material Na-C3N5 of the present invention, compared with Example 1, changes the ratio of sodium chloride to 3-amino-1, 2, 4-triazole, and the preparation method comprises the following steps:

[0043] (1) Sodium chloride, sodium hydroxide and 3-amino-1,2,4-triazole were ground in a mortar in a ratio of 1:0.03:0.5;

[0044] (2) The mixed powder was transferred into a 50 ml crucible and placed in a muffle furnace for calcination at 600 °C, a heating rate of 6 °C / min, and a holding time of 4 h. After the holding time was up, the mixture was cooled to room temperature.

[0045] (3) The obtained brown solid was washed with a large amount of deionized water at a temperature of 80°C; the obtained brown solid aqueous solution was tested with silver nitrate to determine whether the chloride ions were washed away, and the obtained samples were collected, centrifuged, washed, dried, and ground to obtain nanosheets labeled as Na-C3N5-5.

[0046] Example 3

[0047] The reversible photochromic material Na-C3N5 of the present invention, compared with Example 1, changes the ratio of sodium chloride to 3-amino-1, 2, 4-triazole, and the preparation method comprises the following steps:

[0048] (1) Sodium chloride, sodium hydroxide and 3-amino-1,2,4-triazole were ground in a mortar in a ratio of 1:0.02:0.7;

[0049] (2) The mixed powder was transferred into a 50 ml crucible and placed in a muffle furnace for calcination at 600 °C, a heating rate of 6 °C / min, and a holding time of 4 h. After the holding time was up, the mixture was cooled to room temperature.

[0050] (3) Wash the obtained brown solid with a large amount of deionized water at a temperature of 80°C; use silver nitrate to detect whether the chloride ions in the obtained brown solid aqueous solution are washed out, collect the obtained samples, centrifuge, wash, dry, and grind to obtain nanosheets labeled as Na-C3N5-7.

[0051] Comparative Example 1

[0052] The preparation method of C3N5 comprises the following steps:

[0053] Bulk C3N5 was synthesized by a simple thermal polymerization route. 3-Amino-1,2,4-triazole (6 g) was moved to a coffee oven and heated to 500 °C at a heating rate of 5 °C / min, and then kept at this temperature for 3 h. After cooling to room temperature, the sample was placed in a beaker with 100 mL of distilled water and ultrasonicated for 3 h. Next, the sample was treated with deionized water and ethanol to remove the residual precursor, and finally the sample was dried to obtain C3N5 powder.

[0054] Comparative Example 2

[0055] A photochromic material, compared with Example 1, changes the pyrolysis temperature, and the preparation method comprises the following steps:

[0056] (1) Sodium chloride, sodium hydroxide and 3-amino-1,2,4-triazole were ground in a mortar in a ratio of 1:0.03:0.6;

[0057] (2) The mixed powder was transferred into a 50 ml crucible and placed in a muffle furnace for calcination at a temperature of 500 ° C, a heating rate of 6 ° C / min, and a holding time of 4 h. After the time is up, it was cooled to room temperature;

[0058] (3) Wash the obtained brown solid with a large amount of deionized water at a temperature of 80°C; use silver nitrate to detect whether the chloride ions in the obtained brown solid aqueous solution are washed out, collect the obtained samples, centrifuge, wash, dry, and grind to obtain nanosheets labeled as 500-Na-C3N5.

[0059] Comparative Example 3

[0060] A photochromic material, compared with Example 1, changes the pyrolysis temperature, and the preparation method comprises the following steps:

[0061] (1) Sodium chloride, sodium hydroxide and 3-amino-1,2,4-triazole were ground in a mortar in a ratio of 1:0.03:0.6;

[0062] (2) The mixed powder was transferred into a 50 ml crucible and placed in a muffle furnace for calcination at a temperature of 500 ° C, a heating rate of 6 ° C / min, and a holding time of 4 h. After the time is up, it was cooled to room temperature;

[0063] (3) Wash the obtained brown solid with a large amount of deionized water at a temperature of 80°C; use silver nitrate to detect whether the chloride ions in the obtained brown solid aqueous solution are washed out, collect the obtained samples, centrifuge, wash, dry, and grind to obtain nanosheets labeled as 800-Na-C3N5.

[0064] Comparative Example 4

[0065] A photochromic material, compared with Example 1, the ratio of sodium chloride to 3-amino-1, 2, 4-triazole is changed, and the preparation method comprises the following steps:

[0066] (1) Sodium chloride, sodium hydroxide and 3-amino-1,2,4-triazole were ground in a mortar in a ratio of 1:0.03:0.2;

[0067] (2) The mixed powder was transferred into a 50 ml crucible and placed in a muffle furnace for calcination at 600 °C, a heating rate of 6 °C / min, and a holding time of 4 h. After the holding time was up, the mixture was cooled to room temperature.

[0068] (3) Wash the obtained brown solid with a large amount of deionized water at a temperature of 80°C; use silver nitrate to detect whether the chloride ions in the obtained brown solid aqueous solution are washed clean, collect the obtained samples, centrifuge, wash, dry, and grind to obtain nanosheets labeled as Na-C3N5-2.

[0069] Comparative Example 5

[0070] A material, compared with Example 1, the ratio of sodium chloride to 3-amino-1, 2, 4-triazole is changed, and the preparation method comprises the following steps:

[0071] (1) Sodium chloride, sodium hydroxide and 3-amino-1,2,4-triazole were ground in a mortar in a ratio of 1:0.03:1;

[0072] (2) The mixed powder was transferred into a 50 ml crucible and placed in a muffle furnace for calcination at 600 °C, a heating rate of 6 °C / min, and a holding time of 4 h. After the holding time was up, the mixture was cooled to room temperature.

[0073] (3) Wash the obtained brown solid with a large amount of deionized water at a temperature of 80°C; use silver nitrate to detect whether the chloride ions in the obtained brown solid aqueous solution are washed clean, collect the obtained samples, centrifuge, wash, dry, and grind to obtain nanosheets labeled as Na-C3N5-10.

[0074] like Figure 1 As shown, transmission electron microscopy (TEM) was performed on the reversible photochromic material of Example 1. The TEM image clearly shows that the photochromic material is composed of staggered stacks of Na-C3N5 nanosheets, and the product of Example 1 exists as 2D nanosheets with better dispersion and thickness.

[0075] according to Figure 2As shown, Example 1 and the comparative example were characterized by X-ray diffraction (XRD) using a progressive X-ray diffractometer with CuKα radiation having a wavelength of 0.1540558 nm. The powder X-ray diffraction pattern of the sample was collected by θ / 2θ scanning mode. According to the XRD analysis results, the diffraction patterns of C3N5 and Na-C3N5-6 clearly showed two main peaks, corresponding to the (100) diffraction plane of the repeating unit between the extended distance planes and the (002) diffraction plane of the superimposed π-π conjugated aromatic rings. Further enlarging the XRD local image shows that compared with C3N5, the (100) peak of Na-C3N5-6 is shifted to the left, which is due to the change in the diffraction peak caused by the integration of Na ions into the heptazine unit of Na-C3N5-6 for molten salt treatment. Meanwhile, the (002) peak of Na-C3N5-6 is to the right compared with that of C3N5, indicating a smaller interlayer stacking distance, which is due to the stronger π-π interaction between adjacent heptazine layers.

[0076] like Figure 3 As shown, the reversible photochromic material of Example 1 and the comparative example were solid-state 13 C nuclear magnetic resonance (NMR) characterization showed two obvious bands at 156.7 and 164.6 ppm, which can be attributed to C3N and C2N-NH2 in the heptazine unit. For Na-C3N5-6, new peaks appeared at 168 and 137 ppm, which can be attributed to the cyano group (C≡N).

[0077] like Figure 4 As shown, the reversible photochromic material of Example 1 and the comparative example were characterized by FT-IR. Both C3N5 and Na-C3N5-6 showed several characteristic peaks of CN polymer, namely, the heptazine unit (CNC) at 808 cm -1 Out-of-plane bending vibrations and aromatic CN impurities at 1700-1200 cm -1 It is worth noting that Na-C3N5-6 has a stretching vibration at 2179 cm -1 A new peak was found and attributed to the asymmetric stretching vibration of the cyanide group (C≡N). After molten salt treatment, the intensity of the peak increased.

[0078] like Figure 5 As shown, the reversible photochromic material of Example 1 and the comparative example were characterized by FT-IR. Both C3N5 and Na-C3N5-6 showed several characteristic peaks of C, N, and O. Na-C3N5-6 additionally showed a peak attributable to the Na element, confirming the introduction of Na ions.

[0079] like Figure 6The UV-visible absorption spectra of the comparative suspension and the reversible photochromic material of Example 1 at different irradiation times are shown. The UV-visible absorption spectrum of the comparative C3N5 suspension shows little color change after irradiation. The detailed absorption spectrum of the Na-C3N5-6 suspension gradually broadens in the range of 300-600nm, and the main absorption peak in the range of 300-400nm has an obvious broadening effect, indicating that the color has changed significantly during the photochromic process.

[0080] like Figure 7 As shown, digital photos of the reversible photochromic material Na-C3N5-6 reversible photochromic nanosheets at different times of color change and recovery are recorded. As the duration of illumination increases, Na-C3N5-6 changes from yellow to blue within 50 seconds, and after the illumination stops, as the exposure time of the photochromic material to the air increases, the accumulated electrons are gradually consumed by oxygen or recombined with holes, and the color gradually returns to its original color.

[0081] like Figure 8 As shown, the time required for complete color change and recovery of the reversible photochromic nanosheets of all embodiments and comparative examples is recorded. It can be seen that the comparative example C3N5 does not have the ability of photochromic change and recovery, and the time required for complete color change and recovery of Example 1 is significantly shorter than that of other embodiments. Therefore, the mass ratio of sodium chloride, sodium hydroxide and 3-amino-1, 2, 4-triazole is preferably 1: 0.03: 0.6; in contrast, due to the low pyrolysis temperature, the reaction of comparative example 2 may not be fully carried out, resulting in insufficient formation of Na-C3N5 nanosheets. This will result in residual unreacted precursors in the material, or the production of products with low crystallinity. Since these precursors or incompletely reacted compounds cannot effectively form the desired crystal structure, the photochromic properties of the material completely disappear. Comparative example 3 caused the destruction of the nanostructure of Na-C3N5 due to the high pyrolysis temperature. At high temperatures, the chemical bonds in the material may break or reorganize, resulting in the loss of the desired photochromic functional structure. The material may become over-crystallized or sintered, which will reduce the independence and specific surface area of ​​the nanosheets, affecting the absorption of light and the storage process of photoinduced electrons. The small amount of NaCl in Comparative Example 4 will cause the generated Na-C3N5 nanosheets to have an uneven structure and incomplete stacking, resulting in unstable optical properties of the material. Photons cannot propagate effectively in an uneven structure, and the generation and storage process of photoinduced electrons will also be affected, resulting in a decrease in photochromic performance. In Comparative Example 5, although NaCl can promote the formation of carbon nitride nanosheets, excessive template action may cause excessive growth of nanosheets to form an overly thick stacked structure. This will reduce the specific surface area of ​​the material, reduce the effective absorption of light and the separation efficiency of electrons, and thus affect the photochromic performance.

[0082] like Fig. 9As shown, the A / A0 irradiation diagram of the reversible photochromic material Na-C3N5-6 reversible photochromic nanosheet under the optical switch condition, the lower and upper parts respectively represent the changes of the Na-C3N5-6 suspension under the on / off light irradiation at random wavelengths, where A / A0 represents the relative absorption intensity obtained within 60s of irradiation. It can be seen that when the irradiation time reaches 60s, the A / A0 value reaches 100%, and the determination coefficient (R 2 ) is 0.990. During the recovery process, the reversibility of the color change also shows a strong linear relationship during the recovery process (R 2 =0.994).

[0083] like Fig.10 As shown, the unpaired electrons recorded by ESR test under dark / irradiated conditions for the reversible photochromic material Na-C3N5-6. Due to the presence of unpaired electrons in the aromatic ring of the CN part, both clock states show obvious resonance peaks at g = 2.0049. It is worth noting that under irradiated conditions, the Na-C3N5 suspension shows a stronger paramagnetic signal than its dark state, which means that there are additional unpaired electrons in the material. These electrons are believed to be photoexcited and subsequently trapped in the Na-C3N5 suspension accompanied by a change in color.

[0084] like Fig.11 Figure 2 shows a cycling experiment to measure the photochromic response of the reversible photochromic material Na-C3N5-6 reversible photochromic nanosheets. As shown in the figure, even after 8 repeated cycles, the absorbance of the Na-C3N5-6 suspension only slightly decreased, indicating that the color transition has a high reversibility during continuous cycling.

[0085] like Fig.12 As shown, the X-ray diffraction analysis spectra (XRD) of the reversible photochromic material Na-C3N5-6 reversible photochromic nanosheets before and after the color switching were measured. The results showed that there was no change before and after the reaction, confirming its superior stability, which can resist corrosion and thermal decomposition during the color change process, so that Na-C3N5 still shows good stability after multiple cycles of color change.

Claims

1. A reversible photochromic material, characterized in that: The photochromic material is composed of staggered layers of Na-C3N5 nanosheets, wherein the Na-C3N5 nanosheets are obtained by polymerizing sodium chloride and sodium hydroxide with a precursor, and the precursor is 3-amino-1, 2, 4-triazole.

2. The reversible photochromic material according to claim 1, characterized in that: The mass ratio of the sodium chloride, sodium hydroxide and the precursor is 1:0.02-0.05:0.5-0.

8.

3. The reversible photochromic material according to claim 1, characterized in that: The thickness of the Na-C3N5 nanosheet is 4-6nm.

4. A method for preparing the reversible photochromic material according to claim 1, characterized in that: The following steps are involved: (1) mixing sodium chloride, sodium hydroxide and a precursor and grinding them thoroughly to obtain a mixed powder; (2) calcining the mixed powder, and cooling to room temperature to obtain a solid material after the reaction is completed; (3) Washing the solid material with water, centrifuging, washing and drying the solid, and grinding to obtain a medium to reversible photochromic material.

5. The preparation method according to claim 4, characterized in that: In step (2), the calcination treatment is carried out at a temperature of 550 to 600° C., a heating rate of 4 to 6° C. / min, and a holding time of 2.5 to 4.5 h.

6. The preparation method according to claim 4, characterized in that: In step (3), the water washing adopts deionized water, and the water washing temperature is 80-90°C.

7. The preparation method according to claim 4, characterized in that: In step (3), after the solid material is washed with water, the chloride ion content is detected by silver nitrate detection.

8. The preparation method according to claim 4, characterized in that: The concentration of the silver nitrate solution is 0.01M-0.1M.

9. Use of the reversible photochromic material according to claim 1 in the field of photochromism under aerobic conditions.

10. The use according to claim 9, characterized in that: The photochromic field includes decorative materials or information storage materials.