Preparation method and application of high-temperature-resistant ionic polymer organic phosphorescent scintillator
Through the combination of high-temperature resistant ionic polymer salt and aromatic ionic compounds, the problem of the reduction in scintillation efficiency of phosphorescent scintillators at high temperatures is solved, and high-efficiency and long-life phosphorescence is achieved, which is suitable for applications such as temperature monitoring and X-ray imaging.
Patent Information
- Application Number
- CN202411206612.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
AI Technical Summary
Existing phosphorescent scintillator materials exhibit reduced scintillation efficiency and poor durability in high temperature environments, limiting their use in industrial applications, especially radiation monitoring and imaging applications under high temperature conditions.
Using the combination of high-temperature resistant ionic polymer salt and aromatic ionic compounds, the dispersion and ionic interaction of ionic polymer salts can be used to fix guest molecules, limit molecular motion collisions, reduce non-radiative transitions, and achieve high efficiency and long-life phosphorescence. .
It realizes phosphorescence emission that maintains high efficiency at high temperatures, has excellent transparency and high phosphorescence efficiency, is suitable for temperature monitoring, X-ray imaging and anti-counterfeiting ink applications, and maintains phosphorescence performance above 200°C.
Smart Images

Figure CN119081683A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of luminescent materials, and in particular to a high-temperature resistant ionic polymer organic phosphorescent scintillator. Background Art
[0002] Scintillators absorb high-energy (kiloelectronvolt-level) X-ray photons and convert the absorbed energy into lower energy. The ability to convert visible photons is critical for applications in radiation exposure monitoring, safety inspections, X-ray astronomy, and medical radiology. Studies have shown that the properties of the scintillator's atomic composition play an important role in the material's radioluminescence process, because X-ray absorption increases exponentially with atomic number. Although a large number of scintillating materials containing heavy atoms have been characterized in detail as effective X-ray scintillators, almost all of these materials are bulk crystals, which are not conducive to application. It is of great significance to develop high-performance scintillator materials that are low-temperature and solution processable, highly sensitive to X-rays, and can be integrated onto flexible substrates.
[0003] Affected by spin multiplicity, small organic molecules can emit fluorescence from singlet excitons or phosphorescence from triplet excitons. Compared with most current fluorescent scintillators, phosphorescent material scintillators have higher exciton utilization, so they have become a good alternative for developing high-performance scintillators. However, phosphorescence is easily quenched by water and oxygen in the environment, affecting its luminescence efficiency. With the development of this field, room temperature phosphorescent materials have made great progress based on molecular structure design and aggregation behavior modulation, such as enhancing spin-orbit coupling by introducing heavy atoms, improving intersystem crossing efficiency, and using crystal engineering and incorporating amorphous polymers to limit molecular motion collisions and inhibit non-radiative transitions, thereby increasing phosphorescence quantum yield and extending phosphorescence lifetime. Due to the unique property of organic phosphorescent materials that they still have a long-lasting afterglow after excitation, they have good application prospects in biological diagnosis and treatment, light source devices, anti-counterfeiting encryption, etc. However, the preparation conditions of crystalline phosphorescent molecules are complex and the cost is high, which limits the development of phosphorescent materials; and the traditional polymers used for phosphorescent doping have poor air tightness, poor compatibility with organic molecules, and are not resistant to high temperatures, which also greatly limits the industrial application of phosphorescent materials. Inspired by existing research, the entangled structure and long chains of polymers not only ensure a rigid environment for multiple interactions but also protect triplet excitons from the surrounding environment, which is conducive to achieving ultra-long and bright phosphorescent emission. In addition, the environmental tolerance of polymers is also conducive to the practical application of phosphorescent materials. As we all know, phosphorescent luminescence will gradually disappear with increasing temperature, and scintillator materials will also be affected by temperature, resulting in a decrease in scintillation efficiency, which greatly limits the application of organic phosphorescent scintillator materials in high temperature environments. Therefore, it is necessary to develop a new type of high temperature resistant polymer phosphorescent scintillator system so that it can be used under environmental conditions and promote the industrial development of phosphorescent scintillator materials. Summary of the invention
[0004] The object of the present invention is to provide a high temperature resistant ionic polymer organic phosphorescent scintillator.
[0005] Another object of the present invention is to provide a method for preparing a high temperature resistant ionic polymer organic phosphorescent scintillator, so as to prepare the high temperature resistant ionic polymer organic phosphorescent scintillator.
[0006] The present invention also aims to provide an application of a high temperature resistant ionic polymer organic phosphorescent scintillator.
[0007] The technical problem solved by the present invention can be achieved by adopting the following technical solutions:
[0008] The preparation method of a high temperature resistant ionic polymer organic phosphorescent scintillator is characterized in that the ionic polymer salt is used as the main body and the aromatic ionic compound is used as the guest, and the guest molecules are fixed by utilizing the dispersion effect of the ionic polymer salt and the interaction between the ions of the ionic polymer salt and the ions of the aromatic ionic compound, thereby limiting the movement and collision of the guest molecules, reducing non-radiative transitions, and achieving high-efficiency and long-life phosphorescence.
[0009] Preferably, the polymer monomer is used as the starting material, and the polymer is obtained by free radical polymerization. The polymer is treated by acidification to obtain a polymer acid, and then dialyzed and neutralized with alkali to obtain a polymer salt. The polymer monomer includes but is not limited to one or more mixtures of monomers such as styrene, methyl styrene, acrylonitrile, maleic acid, and acrylic acid. The free radical initiator used in the free radical polymerization reaction is a compound with a free radical initiation effect such as benzoyl peroxide, azobisisobutyronitrile, and ammonium persulfate. The acid used in the acidification is various carboxylic acids, sulfuric acid, phosphoric acid and other acidic derivatives. The alkali used in the alkali neutralization is a variety of basic compounds such as sodium hydroxide, potassium hydroxide, magnesium hydroxide, and calcium hydroxide.
[0010] Further preferably, the polymer monomer is styrene. Styrene is polymerized by benzoyl oxide under heating conditions to obtain polystyrene, polystyrene is sulfonated and dialyzed by sulfuric acid to obtain polystyrene sulfonic acid, an equimolar ratio of sodium hydroxide is added to neutralize, and the solvent is evaporated to obtain polystyrene sulfonic acid sodium salt. Polysodium maleate, sodium polyacrylate, sodium polystyrene carboxylate, sodium poly-3-bromostyrene sulfonate, etc. can be prepared based on a similar method.
[0011] Preferably, the polymer salt is prepared by modifying the polymer side chain, including but not limited to polymer sodium salt, potassium salt, calcium salt, etc.
[0012] Preferably, halogen atoms such as F, Cl, Br, etc. are introduced by modifying the polymer main chain or side chain. The heavy atom effect is used to enhance the self-selective coupling and promote phosphorescence, including but not limited to the modification of the polymer main chain and side chain. The structure is shown below:
[0013]
[0014] Wherein R is various salts as described in claims 2-3, and X is a halogen atom such as F, Cl, Br, etc.
[0015] The structure of the aromatic ionic compound includes but is not limited to one or more of the following structural formulas or their similar aromatic structural derivatives:
[0016]
[0017]
[0018] In the formula, X- is independently selected from -COO - 、-SO3 2- ,-PO4 3- One of; G- is independently selected from -Na + , -K + , -Mg 2+ , -Ca 2+ One of the following: R is selected from H, F, Cl, Br or other groups.
[0019] Preferably, the aromatic ionic compound is a condensed aromatic hydrocarbon containing multiple benzene rings. Its larger conjugated structure and π-π stacking are advantageous for opening more intersystem crossing channels, and the introduction of carbonyl groups using carboxylate anions as an example promotes intersystem crossing efficiency with a higher triplet exciton yield, providing basic conditions for achieving high-brightness phosphorescence.
[0020] The high temperature resistant ionic polymer organic phosphorescent scintillator can continuously blue-shift its wavelength as the temperature rises, thus realizing the monitoring of different temperatures. Therefore, it can be used for temperature monitoring.
[0021] High temperature resistant ionic polymer organic phosphorescent scintillator has high transparency and high phosphorescence efficiency, so it can be used for X-ray imaging and non-destructive testing of human tissue.
[0022] High temperature resistant ionic polymer organic phosphorescent scintillator can be well dispersed in aqueous solution, so it can be used as anti-counterfeiting ink for information encryption.
[0023] High temperature resistant ionic polymer organic phosphorescent scintillators can also be used in OLED, damage detection, etc.
[0024] Beneficial effects:
[0025] 1. The present invention utilizes the polymer salt entanglement structure and long chains to ensure a rigid environment with multiple interactions, which can better disperse the aromatic ionic compound guests and effectively reduce the triplet-triplet quenching between the guest molecules.
[0026] 2. The present invention utilizes the ionic interaction between the polymer salt host and the aromatic ionic guest to fix the guest molecules, limit the movement and collision of the guest molecules, reduce non-radiative transitions, and achieve high-efficiency and long-life phosphorescence.
[0027] 3. The present invention is based on the salt formation of polymer, which greatly improves the melting point of the polymer, so that the phosphorescent system still has excellent phosphorescent properties at high temperatures.
[0028] 4. The high temperature resistant ionic polymer organic phosphorescent scintillator of the present invention is easy to prepare. Specifically, the polymer monomer is very common, cheap and easy to obtain, the preparation process is simple, and the yield is high, which is conducive to industrial production. Secondly, based on the ionic interaction between the polymer salt host and the aromatic ionic guest, it is conducive to reducing molecular motion collisions, reducing non-radiative transitions, and achieving high-efficiency and long-life phosphorescence, which is conducive to its application as an X-ray scintillator for imaging.
[0029] 5. The high temperature resistant ionic polymer organic phosphorescent scintillator of the present invention can be well dispersed in an aqueous solution and used as an anti-counterfeiting ink for information encryption.
[0030] 6. The high temperature resistant ionic polymer organic phosphorescent scintillator of the present invention still has phosphorescent luminescence performance at a high temperature exceeding 200°C, and exhibits a wavelength blue shift as the temperature changes, thereby realizing temperature monitoring. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The drawings in the specification, which constitute a part of this application, are used to provide a further understanding of the present invention. The illustrative embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0032] Figure 1 , are the steady-state (left) and phosphorescence (right) spectra of the high-temperature resistant ionic polymer organic phosphorescent scintillator material film at 30°C in the specific implementation case 1, with the horizontal axis being the wavelength (nm) and the vertical axis being the intensity.
[0033] Figure 2 , is a phosphorescence lifetime diagram of the high temperature resistant ionic polymer organic phosphorescent scintillator material film at 30°C in the specific implementation case 1, where the horizontal axis is time (s) and the vertical axis is the number of photons.
[0034] Figure 3 , is the phosphorescence spectrum of the high temperature resistant ionic polymer organic phosphorescent scintillator material film in the specific implementation case 1 when the ambient temperature rises from 30°C to 320°C, the abscissa is the wavelength (nm) and the ordinate is the intensity.
[0035] Figure 4 , is a photo of the afterglow of the high temperature resistant ionic polymer organic phosphorescent scintillator material film in the specific implementation case 1 after the ultraviolet lamp is turned off when the ambient temperature rises from 30°C to 320°C.
[0036] Figure 5 , For the specific implementation case 2, the anti-counterfeiting ink was prepared using high-temperature resistant ionic polymer organic phosphorescent scintillator material, and the afterglow photograph was taken after the ultraviolet lamp was turned off when the ambient temperature increased from 100°C to 400°C.
[0037] Figure 6 , is the luminescence spectrum of the high temperature resistant ionic polymer organic phosphorescent scintillator material film in the specific implementation case 1 after X-ray excitation.
[0038] Figure 7 , is the X-ray imaging of the high temperature resistant ionic polymer organic phosphorescent scintillator material film at different temperatures in the specific implementation case 1. DETAILED DESCRIPTION
[0039] The present invention is further described below by way of examples, the purpose of which is only to provide a better understanding of the content of the present invention. Therefore, the examples given do not limit the scope of protection of the present invention:
[0040] like Figure 1-7 It should be noted that the structures, proportions, sizes, etc. illustrated in the drawings of this specification are only used to match the contents disclosed in the specification, so that people familiar with this technology can understand and read, and are not used to limit the limiting conditions that the present invention can implement. Any modification of the structure, change of the proportional relationship or adjustment of the size are not technically significant. The following examples are provided to better understand the present invention, but are not intended to limit the present invention. The experimental methods in the following examples are conventional methods unless otherwise specified. The experimental materials used in the following examples are all purchased from conventional biochemical reagent stores unless otherwise specified.
[0041] Unless otherwise specified, the reagents or materials described in the following examples are commercially available.
[0042] Example 1 (sodium polystyrene sulfonate + potassium coronene tetracarboxylate)
[0043] Preparation method of ionic polymer salt:
[0044] A polymer monomer such as styrene is used as the starting material, dissolved in N,N-dimethylformamide solvent, and 1% by mass of a free radical initiator benzoyl peroxide is added. Under nitrogen protection, the reaction is carried out at 80°C for 12 hours. After the reaction is completed, the reaction solution is added dropwise into a large amount of methanol. The precipitated solid is washed several times and then collected by centrifugation. After dialysis, solid polystyrene is obtained with a yield of 90%.
[0045] Add polystyrene to dichloroethane and heat at 50°C until the polystyrene is completely dissolved for later use; inject acetic anhydride into dichloroethane, and inject concentrated sulfuric acid under ice bath to obtain acetyl sulfate solution, add the solution to the above polymer solution, react at 50°C for 12 hours, the molar ratio of polystyrene:acetyl sulfonate is 9.6:67, the crude product is purified by dialyzing for 24 hours, and evaporated to remove water to obtain sulfonated polystyrene with a yield of 99%.
[0046] Dissolve sulfonated polystyrene in water and add sodium hydroxide in equal molar ratio, stir at room temperature for 12 hours, evaporate and remove water to obtain sodium polystyrene sulfonate with a yield of 99%. The schematic diagram of the synthesis route is as follows:
[0047]
[0048] The polymer monomers may include, but are not limited to, a mixture of one or more monomers such as styrene, methyl styrene, methacrylic acid, maleic acid, acrylic acid, etc. The structure is shown below:
[0049]
[0050] Wherein R is various carboxylates, sulfates, phosphates, etc.
[0051] Polymer salts can be prepared by modifying the polymer side chains, including but not limited to polymer sodium salts, potassium salts, calcium salts, etc. It is also possible to introduce halogen atoms such as F, Cl, Br, etc. by modifying the polymer main chain or side chain, and utilizing the heavy atom effect to enhance the self-selective coupling and promote phosphorescence, including but not limited to polymer main chain and side chain modification, etc. Its structure is shown below:
[0052]
[0053] Wherein R is carboxylate, sulfate, sodium phosphate, potassium salt, calcium salt, etc., and X is a halogen atom such as F, Cl, Br, etc.
[0054] Preparation method of aromatic ionic compounds: According to existing literature, coronet tetraethyl ester is synthesized, dissolved in ethanol, and an excess of potassium hydroxide is added for hydrolysis, heated under reflux for 12 hours, and after the reaction is completed, hydrochloric acid is added to adjust the pH and poured into water for centrifugation to obtain coronet tetracarboxylic acid with a yield of 90%; coronet tetracarboxylic acid is dissolved in THF, and an equal molar ratio of high-purity potassium hydroxide is added and stirred at room temperature for 12 hours, and the solvent is evaporated to obtain potassium coronet tetracarboxylate with a yield of 99%. The specific synthesis route is as follows:
[0055]
[0056] Aromatic ionic compounds, whose structures include but are not limited to one or more of the following structural formulas:
[0057]
[0058]
[0059] In the formula, X- is independently selected from -COO - 、-SO3 2- ,-PO4 3- One of; G- is independently selected from -Na + , -K + , -Mg 2+ , -Ca 2+ One of the following: R is selected from H, F, Cl, Br or other groups.
[0060] Preparation method of high temperature resistant ionic polymer organic phosphorescent scintillator:
[0061] 1 mg of potassium coronene tetracarboxylate aromatic ion guest compound and 100 mg of sodium polystyrene sulfonate host polymer were dissolved in 2 mL of water at the same time, ultrasonically dissolved, vortex mixed, and dried in an oven at 75° C. for 3 h to prepare a polymer phosphorescent film with high transparency.
[0062] The steady-state spectrum, phosphorescence spectrum, and phosphorescence lifetime were all recorded by FLS1000wen spectrometer, and the photos were taken by Canon800D.
[0063] Different monomers can be selected for copolymerization to enrich the intermolecular / intramolecular interactions within the polymer to suppress the construction of a rigid environment for non-radiative inactivation. Interactions such as ionic bonds, hydrogen bonds, and covalent bonds can change the electronic structure of the molecule and affect the energy dissipation channel of the excited state.
[0064] Different monomers can be selected to copolymerize with polycyclic aromatic hydrocarbons to enrich the singlet and triplet energy levels inside the polymer, which is conducive to opening more intersystem crossing channels and enhancing phosphorescence efficiency. Its structural formula is as follows:
[0065]
[0066] Different monomers can be selected to copolymerize with carbonyl compounds, which is beneficial to improve the intersystem crossing efficiency and enhance phosphorescence. The structure is shown below:
[0067]
[0068] Wherein R is various salts as described in claims 2-3, and X is an atom such as H, F, Cl, Br, etc.
[0069] Example 2: Preparation method of anti-counterfeiting ink:
[0070] 1 mg of potassium coronene tetracarboxylate aromatic ion guest compound and 100 mg of sodium polystyrene sulfonate host polymer were dissolved in 5 mL of water at the same time, ultrasonically dissolved, and vortex mixed to prepare a phosphorescent anti-counterfeiting ink with high transparency. The ink was written on ordinary paper, and the light color changed differently at different temperatures.
[0071] The spectrum and application effects of high temperature resistant ionic polymer organic phosphorescent scintillator are as follows Figure 1-7 shown.
[0072] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the design strategy or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A method for preparing a high temperature resistant ionic polymer organic phosphorescent scintillator, characterized in that: Taking ionic polymer salt as the main body and aromatic ionic compound as the guest, the dispersing effect of ionic polymer salt and the interaction between ions of ionic polymer salt and ions of aromatic ionic compound are utilized to fix the guest molecules, limit the movement and collision of guest molecules, reduce non-radiative transitions, and achieve high-efficiency and long-life phosphorescence.
2. The method for preparing the high temperature resistant ionic polymer organic phosphorescent scintillator according to claim 1, characterized in that: The polymer monomer is used as the starting material, and a polymer is obtained through free radical polymerization reaction. The polymer is subjected to acidification treatment to obtain a polymer acid, which is dialyzed and then neutralized with an alkali to obtain a polymer salt.
3. The method for preparing the high temperature resistant ionic polymer organic phosphorescent scintillator according to claim 2, characterized in that: The polymer monomer is a mixture of one or more of styrene, methyl styrene, acrylonitrile, maleic acid and acrylic acid.
4. The method for preparing a high temperature resistant ionic polymer organic phosphorescent scintillator according to claim 2, characterized in that: The free radical initiator used in the free radical polymerization reaction is benzoyl peroxide, azobisisobutyronitrile or ammonium persulfate.
5. The method for preparing the high temperature resistant ionic polymer organic phosphorescent scintillator according to claim 2, characterized in that: The acid used for acidification is carboxylic acid, sulfuric acid or phosphoric acid.
6. The method for preparing a high temperature resistant ionic polymer organic phosphorescent scintillator according to claim 2, characterized in that: The alkali used for alkali neutralization is sodium hydroxide, potassium hydroxide, magnesium hydroxide or calcium hydroxide.
7. The method for preparing a high temperature resistant ionic polymer organic phosphorescent scintillator according to claim 1, characterized in that: The structural formula of the ionic polymer salt is any one of the following structural formulas: Wherein R is one of carboxylate, sulfate and phosphate; X is a halogen atom.
8. The method for preparing a high temperature resistant ionic polymer organic phosphorescent scintillator according to claim 1, characterized in that: The structural formula of the aromatic ionic compound is any one of the following structural formulas: In the formula, X- is -COO - 、-SO3 2- ,-PO4 3- One of them; G- is -Na + , -K + , -Mg 2+ , -Ca 2+ R is one of H, F, Cl, and Br.
9. Application of the high temperature resistant ionic polymer organic phosphorescent scintillator prepared by the method for preparing the high temperature resistant ionic polymer organic phosphorescent scintillator according to any one of claims 1 to 8, characterized in that: For temperature detection, X-ray imaging or anti-counterfeiting inks.
10. The use of the high temperature resistant ionic polymer organic phosphorescent scintillator according to claim 9, characterized in that: 1 mg of potassium coronene tetracarboxylate aromatic ion guest compound and 100 mg of sodium polystyrene sulfonate host polymer were dissolved in 5 mL of water at the same time, ultrasonically dissolved, and vortex mixed to obtain a phosphorescent anti-counterfeiting ink with high transparency.