Method and system for preventing ladle adhesion in casting residue return production process
By installing a baking device on the molten iron bag and using the descent truck to reduce heat loss, the problem of sticking caused by the molten iron bag cooling in the casting residue recycle production process is solved, and the high-temperature state maintenance and environmental protection efficiency of the casting residue are achieved.
Patent Information
- Application Number
- CN202310661269.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-06
- Publication Date
- 2024-12-06
AI Technical Summary
In the casting residue return production process, the molten iron bag is prone to cooling during the waiting and receiving the casting residue, resulting in heat loss, resulting in the casting residue and the molten iron bag wall bonding to the condensation slag. The existing technology lacks an effective solution.
By installing a lid equipped with a baking device on the molten iron bag and using a defensive truck during the transfer process to reduce heat loss, the baking device is used to keep the molten iron bag and cast residue in a high temperature state, avoiding the sticking phenomenon caused by temperature drop.
It effectively prevents the problem of sticking the residual slag in the molten iron bag, realizes the high-temperature state of the residual slag, reduces the impact of on-site logistics, and improves the productivity and environmental benefits of steelmaking.
Smart Images

Figure CN119082383A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of recycling of steel smelting slag, and in particular to a method and a system for preventing a molten iron ladle from sticking in a casting slag recycling production process. Background Art
[0002] In the casting slag recycling process, the key development point is to return the ladle to the production process after receiving multiple bags of casting slag for reuse. Usually, the ladle pre-loaded with a portion of hot molten iron needs to wait for a period of time after arriving at the station to receive the casting slag. After the molten steel is poured, the casting slag in the steel ladle is loaded into the ladle, and the casting slag reacts with the molten iron and absorbs heat from the mixed melt. The time interval from the first time the ladle receives the casting slag to the next time it receives the casting slag is generally about 30 minutes, and it is waiting in an open state, which will cause the melt in the ladle to cool down during the waiting time and lose the heat of the system.
[0003] After the ladle has received casting slag for many times, if the heat brought in by the poured casting slag is not enough to make up for the heat absorbed by the reaction between the casting slag and molten iron and the heat lost during the waiting period of the ladle receiving the casting slag, the temperature of the casting slag layer in the ladle will drop a little each time the ladle receives the casting slag. After the ladle has received casting slag for many times, the casting slag at the top layer will stick to the wall of the ladle due to the excessive temperature drop and solidify into slag.
[0004] In the casting slag recycling process, there is a problem of slagging and sticking of casting slag in the ladle. Since the technology is still under development, there is no effective and mature solution. Currently, it can only be avoided by frequent observation and reducing the number of times the ladle takes on casting slag during production. Summary of the invention
[0005] The purpose of the present invention is to provide a method and system for preventing the ladle from sticking in the casting slag recycling production process, solve the problem of slag sticking to the ladle wall during the casting slag recycling production process, promote the full implementation of the casting slag recycling production process, and have significant economic and environmental benefits.
[0006] To achieve the above object, the technical solution of the present invention is:
[0007] A method for preventing ladle sticking in a casting slag recycling process, comprising the following steps:
[0008] 1) After the molten iron is loaded into the ladle for standby use, the amount of molten iron loaded is 10-15% of the molten iron volume, and the ladle filled with molten iron is called a heavy ladle. The ladle is equipped with a ladle cover of matching size and shape, and a baking device is installed on the ladle cover; a trolley that can move back and forth is set between the molten steel receiving span and the charging span, and a baking station is set in the molten steel receiving span;
[0009] 2) The heavy ladle is hoisted onto the span trolley, and then the span trolley is opened from the charging span to the molten steel receiving span. After that, the heavy ladle is hoisted from the span trolley, placed at the baking station, and the ladle cover is placed on the heavy ladle, and baked to the set temperature;
[0010] 3) After the molten steel is poured, the ladle cover is opened, the casting slag in the ladle is poured into the heavy ladle, and the ladle cover is covered on the heavy ladle again. The heavy ladle is baked to a set temperature and then kept warm until the heavy ladle receives the casting slag again, and the above operation is repeated until the heavy ladle receives the casting slag;
[0011] 4) After the heavy ladle has finished taking in the casting slag, it will be hoisted onto the cross-span trolley and transported back to the charging span by the molten steel receiving span. After that, the heavy ladle will be filled with molten iron and returned to the smelting furnace for use.
[0012] Preferably, the baking setting temperature is 1100±20°C.
[0013] In the method of the present invention:
[0014] The present invention arranges a back-and-forth trolley between the charging span and the molten steel receiving span to ensure that after the heavy-clad iron ladle has completed receiving the casting slag, the heavy-clad iron ladle is transferred to the charging span by the back-and-forth trolley. The whole operation process takes the shortest time and can minimize the heat loss of the casting slag.
[0015] The present invention improves the ladle before processing, and is equipped with a ladle cover that matches the size and shape of the ladle opening. The ladle cover is placed on the ladle opening to form a full envelope of the ladle opening, thereby avoiding heat dissipation during baking and heat preservation. In addition, a baking device and a temperature monitoring device are provided on the ladle cover. When the temperature of the ladle is lower than the set temperature, the baking device is turned on. After the temperature in the ladle reaches the set temperature, the baking device is turned off to start heat preservation and stewing. In this way, the ladle wall and the cover are always kept at a high temperature. In addition, the baking device is arranged on the ladle cover, and during the baking process, the temperature is directly transferred to the surface casting slag, thereby avoiding slagging of the surface casting slag due to the temperature reduction, and effectively preventing the casting slag from sticking in the ladle.
[0016] The present invention reduces heat loss during the transfer process by arranging a transfer trolley that moves back and forth between the charging span and the molten steel receiving span. In addition, by baking the molten iron ladle and the casting slag, heat is further supplemented to the casting slag, so that the molten iron ladle and the casting slag are kept in a high temperature state in the receiving gap, effectively avoiding the temperature drop of the casting slag contained in the molten iron ladle, and preventing the occurrence of the molten iron ladle sticking after the molten iron ladle receives the casting slag for multiple times.
[0017] The present invention also provides a system for preventing ladle sticking in a casting slag recycling process, which comprises:
[0018] Feed span;
[0019] A molten steel receiving span is arranged in parallel with the charging span, and at least one baking station is arranged in the molten steel receiving span;
[0020] A cross-span trolley that can move back and forth between the molten steel receiving span and the charging span;
[0021] A plurality of ladles and ladles covers, wherein the ladles are arranged in the feeding span; and a baking device and a temperature monitoring device are arranged on the ladles covers.
[0022] Furthermore, it also includes a cover-adding mechanism, which is arranged in the molten steel receiving span and cooperates with the molten iron ladle.
[0023] Preferably, the baking device is a gas baking device, which is provided with a plurality of gas baking burners.
[0024] Preferably, the excess air coefficient of the gas baking burner is 0.95-1.02.
[0025] Preferably, both the charging span and the molten steel receiving span are equipped with cranes.
[0026] Preferably, two baking stations are arranged in the molten steel receiving span, or one baking station and one temporary parking station are arranged.
[0027] A baking station is set up in the molten steel receiving bay. At least one baking station is set up. When there are more than two baking stations, one baking station is used to place the ladle that is receiving the casting slag. The other baking station is used to place the spare ladle pre-loaded with molten iron. After the previous ladle has finished receiving the casting slag and has been transported away, the spare ladle on this baking station starts to be used to receive the casting slag.
[0028] Alternatively, a baking station and a temporary parking station for the ladle are set up. The ladle on the baking station is receiving the casting slag, and the spare ladle pre-filled with molten iron that is transported from the charging span is placed at the temporary parking station for standby. After the ladle on the baking station has completed receiving the casting slag and transported it away, the spare ladle is transferred to the baking station and put into use.
[0029] The baking device is a gas baking device, which is composed of a plurality of gas baking burners. The excess air coefficient of the gas baking burner is set to 0.95-1.02. A smaller excess air coefficient is used to keep the outlet flame atmosphere weakly reducing or neutral, which can better protect the ladle lining.
[0030] The lid of the ladle is controlled by the lid-lifting mechanism. When the ladle needs to be baked, the molten steel receiving straddle crane lifts the ladle to the baking station and puts it there. The lid-lifting mechanism covers the ladle and ignites the fire to start baking. When the slag is to be received, the baking is stopped in advance, and the lid of the ladle is removed from the ladle by the lid-lifting mechanism to facilitate the pouring of the slag into the ladle. After the pouring of the slag is completed, the lid of the ladle is put back on the ladle for baking or heat preservation.
[0031] The differences and improvements of the present invention over the prior art are as follows:
[0032] Chinese patent CN2018102072178 discloses "a method for recovering molten steel by returning hot casting slag to a ladle", which receives and circulates multiple ladles of casting slag by means of a holding furnace arranged in the molten steel receiving span. The function of the holding furnace is to heat the casting slag by induction heating or oxygen blowing, and at least three ladles of casting slag are poured into the ladles. Since the casting slag is a poor conductor of heat, the thick slag layer cannot be heated regardless of induction heating or oxygen blowing. The slag layer on the upper surface will also cool down and solidify, and will not play the role of heating or heat preservation of the slag. The present invention reduces the heat dissipation in the process on the one hand by improving the transfer process and the ladle cover, and on the other hand, the ladle cover with a baking device can directly heat the surface casting slag during the baking process, so that the ladle wall and the casting slag are always kept at a high temperature, thereby avoiding the slag slagging.
[0033] Chinese patent CN2018115574613 discloses "a method for recycling hot casting slag from ladle in converter", step 1): after the converter taps steel, the converter slag is splashed in the converter, and the converter slag is splashed and all of it remains in the converter, located at the bottom and lining of the converter; step 2): the hot metal is desulfurized and pretreated in the molten iron tank, and the hot casting slag is mixed with the molten iron after slagging and added to the converter for converter smelting. After the molten iron is pretreated and slag is removed, the temperature of the molten iron will be greatly reduced, and then the casting slag is directly poured into it. The further reaction of the casting slag and the molten iron will absorb heat, so the casting slag is easy to stick to the ladle. When pouring molten iron to the converter, the slag on the wall of the molten iron ladle will make it difficult to predict the path, direction and speed of the molten iron being poured into the converter. It is very likely that the molten iron and slag will splash everywhere, or even splash out of the converter, which will bring great danger to the operation of adding molten iron to the converter.
[0034] Chinese patent CN2010102764524 discloses "a method for recycling and reusing hot slag from continuous casting ladle". In continuous casting production, after the ladle molten steel is injected into the tundish, the molten hot slag in the ladle is poured into the heavy iron tank; then the hot slag is added to the converter together with the molten iron for steelmaking. The patent mentions that the slag may coagulate, but no solution is proposed. The present invention focuses on how to prevent the casting slag from coagulating due to continuous cooling.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] 1. On the one hand, the present invention reduces the heat dissipation in the gap between the ladle and the casting slag by improving the transfer process and equipment, and on the other hand, uses the ladle cover with a baking device to bake, always maintaining the high temperature state of the casting slag and the ladle wall in the heavy ladle, compensating for the temperature drop caused by the heat dissipation and the heat absorption of the slag-iron reaction, thereby avoiding the problem of the casting slag sticking due to the excessive temperature drop. One ladle can receive multiple packages of casting slag and then return them to production, which greatly reduces the impact on on-site logistics and scheduling, and can realize the large-scale return of casting slag to production.
[0037] 2. The method of the present invention not only allows the casting slag to be recycled in a hot state within the steel plant process, but also allows the heat of the non-metallic slag therein to be recycled and effectively utilized, which greatly improves the steelmaking productivity and reduces the energy consumption and cost of the steelmaking process.
[0038] 3. Compared with the existing more advanced casting slag grid treatment process, it avoids the long process and serious pollution problems in the existing casting slag treatment process, realizes the clean production of the steelmaking process, and greatly reduces the cost of slag treatment, promoting the realization of circular economy and green factory in steel plant. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is a process layout diagram of Example 1 of the method of the present invention;
[0040] Figure 2 This is a process layout diagram of Example 2 of the method of the present invention;
[0041] Figure 3 This is a process layout diagram of Example 3 of the method of the present invention;
[0042] Figure 4 It is a schematic diagram of a heavy iron ladle being baked at a baking station according to an embodiment of the present invention;
[0043] Figure 5 It is a schematic diagram of a heavy-clad iron ladle receiving casting slag in an embodiment of the present invention. DETAILED DESCRIPTION
[0044] See also Figure 1 to Figure 5 The system for preventing the ladle from sticking in the casting slag recycling process of the present invention comprises:
[0045] Feed span 1;
[0046] The molten steel receiving span 2 is arranged in parallel with the charging span 1, and at least one baking station 3 is arranged in the molten steel receiving span 2.
[0047] A cross-span trolley 4, which can move back and forth between the molten steel receiving span 2 and the charging span 1;
[0048] A plurality of ladles 5 and ladles covers 6 are provided. The ladles 5 are arranged in the charging span 1. The ladles covers 6 are provided with a baking device 7 and a temperature monitoring device.
[0049] Furthermore, it also includes a cover-adding mechanism 8, which is arranged in the molten steel receiving span 2 and cooperates with the molten iron ladle 5.
[0050] Preferably, the baking device 7 is a gas baking device, which is provided with a plurality of gas baking burners 71 .
[0051] Preferably, the feeding span 1 and the molten steel receiving span 2 are respectively provided with a crane 9 and a crane 10.
[0052] Preferably, two baking stations 3 and 3' are arranged in the molten steel receiving bay 2, or one baking supply station 3 and a temporary parking station 11 are arranged.
[0053] Example 1
[0054] See also Figure 1 , Figure 4 , Figure 5 A method for preventing ladle sticking in a casting slag recycling process comprises the following steps:
[0055] 1) After the molten iron is loaded into the ladle for standby use, the amount of molten iron loaded is 10% of the amount of molten iron contained in the ladle, and the ladle filled with molten iron is called a heavy ladle 5, the ladle is equipped with a ladle cover 6 of matching size and shape, and the ladle cover 6 is provided with a baking device 7; a trolley 4 that can move back and forth is set between the molten steel receiving span 2 and the charging span 1, and a baking station 3 is set in the molten steel receiving span;
[0056] 2) The heavy ladle 5 is hoisted onto the over-span trolley 4 by the crane 9 in the charging span, and then the over-span trolley 4 is driven from the charging span 1 to the molten steel receiving span 2. The heavy ladle 5 is then hoisted down from the over-span trolley 4 by the crane 10 in the molten steel receiving span, and placed in the baking station 3. The ladle cover 6 is covered on the heavy ladle 5 by the cover-uncovering mechanism 8, and baked to 1100°C;
[0057] 3) After the molten steel is poured, the ladle cover 6 is opened by the cover-lifting mechanism 8, and the casting slag in the ladle 100 is poured into the heavy ladle 5. The ladle cover 6 is covered on the heavy ladle 5 by the cover-lifting mechanism 8 again, and the heavy ladle 5 is baked to 1100° C. until the heavy ladle 5 receives the casting slag again. The above operation is repeated until the heavy ladle 5 receives the casting slag.
[0058] 4) After the heavy ladle 5 has finished receiving the casting slag, the crane 10 in the molten steel receiving span 2 is used to lift the heavy ladle 5 onto the crossing trolley 4 and transport it back to the charging span 1 via the molten steel receiving span 2. After that, the heavy ladle 5 is filled with molten iron and returned to the smelting furnace for use.
[0059] Example 2
[0060] See also Figure 2 , Figure 4 , Figure 5 A method for preventing ladle sticking in a casting slag recycling process comprises the following steps:
[0061] 1) After the molten iron is loaded into the ladle for standby use, the amount of molten iron loaded is 10% of the molten iron capacity, and the ladle filled with molten iron is called a heavy ladle 5, the ladle is equipped with a ladle cover 6 of matching size and shape, and a baking device 7 is provided on the ladle cover; a trolley 4 that can move back and forth is set between the molten steel receiving span 2 and the charging span 1, and baking stations 3 and 3' are set in the molten steel receiving span 2;
[0062] 2) The heavy ladle 5 is hoisted onto the over-span trolley 4 by the crane 9 in the charging span 1, and then the over-span trolley 4 is driven from the charging span 1 to the molten steel receiving span 2. The heavy ladle 5 is then hoisted down from the over-span trolley 4 by the crane 10 in the molten steel receiving span 2, and placed in the baking station 3. The ladle cover 6 is covered on the heavy ladle 5 by the cover-uncovering mechanism 8, and baked to 1080°C;
[0063] 3) After the molten steel is poured, the ladle cover 6 is opened, and the casting slag in the ladle 100 is poured into the heavy ladle 5, and the ladle cover 6 is covered on the heavy ladle 5 again, and the heavy ladle 5 is baked to 1080° C. until the heavy ladle 5 receives the casting slag again, and the above operation is repeated until the heavy ladle 5 receives the casting slag; in the process of the heavy ladle 5 receiving the casting slag, the overturning trolley 4 transfers another heavy ladle from the feeding span 1 to the molten steel receiving span 2, and the heavy ladle 5 is placed on another baking station 3' in the molten steel receiving span 2 for baking. After the previous heavy ladle 5 receives the casting slag, the heavy ladle 5 starts to be put into use;
[0064] 4) Casting slag transfer
[0065] After the heavy ladle 5 has completed receiving the casting slag, the crane 10 in the molten steel receiving span is used to lift the heavy ladle 5 onto the crossing trolley 4 and transported back to the charging span 1 via the molten steel receiving span 2. After that, the heavy ladle 5 is filled with molten iron and returned to the smelting furnace for use.
[0066] Example 3
[0067] See also Figure 3 , Figure 4 , Figure 5 A method for preventing ladle sticking in a casting slag recycling process comprises the following steps:
[0068] 1) After the molten iron is loaded into the ladle for standby use, the amount of molten iron loaded is 10% of the amount of the molten iron container, and the ladle filled with molten iron is called a heavy ladle 5, the ladle is equipped with a ladle cover 6 of matching size and shape, and the ladle cover is provided with a baking device 7; a trolley 4 that can move back and forth is set between the molten steel receiving span 2 and the charging span 1, and a baking station 3 and a temporary parking station 11 are set in the molten steel receiving span 2;
[0069] 2) The heavy ladle 5 is hoisted onto the over-span trolley 4 by the crane 9 in the charging span 1, and then the over-span trolley 4 is driven from the charging span 1 to the molten steel receiving span 2. After that, the heavy ladle 5 is hoisted down from the over-span trolley 4 by the crane 10 in the molten steel receiving span 2, and placed in the baking station 3, and the ladle cover 6 is covered on the heavy ladle 5, and baked to 1120°C;
[0070] 3) After the molten steel is poured, the ladle cover 6 is opened, and the casting slag in the ladle 100 is poured into the heavy ladle ladle 5, and the ladle cover 6 is covered on the heavy ladle ladle 5 again, and the heavy ladle ladle 5 is baked to 1080° C. until the heavy ladle ladle 5 receives the casting slag again, and the above operation is repeated until the heavy ladle ladle 5 receives the casting slag. In the process of the heavy ladle ladle 5 receiving the casting slag, the overturning trolley 4 transfers another heavy ladle ladle from the feeding span 1 to the molten steel receiving span 2, and the heavy ladle ladle 5 is placed in the temporary parking station 11 in the molten steel receiving span 2;
[0071] 4) After the heavy-clad iron ladle 5 has completed receiving the casting slag, the crane 10 in the molten steel receiving span 2 is used to lift the heavy-clad iron ladle 5 onto the crossing trolley 4 and transported back to the charging span 1 from the molten steel receiving span 2. After that, the heavy-clad iron ladle 5 is filled with molten iron and returned to the smelting furnace for use. The heavy-clad iron ladle 5 on the temporary parking station 11 is transferred to the baking station 3 to start baking and put into use, and the operation is repeated in this way.
Claims
1. A method for preventing ladle sticking in a casting slag recycling process, characterized in that: The steps include: 1) After the molten iron is loaded into the ladle for standby use, the amount of molten iron loaded is 10-15% of the molten iron volume, and the ladle filled with molten iron is called a heavy ladle. The ladle is equipped with a ladle cover of matching size and shape, and a baking device is installed on the ladle cover; a trolley that can move back and forth is set between the molten steel receiving span and the charging span, and a baking station is set in the molten steel receiving span; 2) The heavy ladle is hoisted onto the span trolley, and then the span trolley is opened from the charging span to the molten steel receiving span. After that, the heavy ladle is hoisted from the span trolley, placed at the baking station, and the ladle cover is placed on the heavy ladle, and baked to the set temperature; 3) After the molten steel is poured, the ladle cover is opened, the casting slag in the ladle is poured into the heavy ladle, and the ladle cover is covered on the heavy ladle again. The heavy ladle is baked to a set temperature and then kept warm until the heavy ladle receives the casting slag again, and the above operation is repeated until the heavy ladle receives the casting slag; 4) After the heavy ladle has finished taking in the casting slag, it will be hoisted onto the cross-span trolley and transported back to the charging span by the molten steel receiving span. After that, the heavy ladle will be filled with molten iron and returned to the smelting furnace for use.
2. The method for preventing ladle sticking in the casting slag recycling process according to claim 1, characterized in that: The set temperature of the ladle after baking is 1100±20°C.
3. A system for preventing ladle sticking in the casting slag recycling process as claimed in claim 1, characterized in that: include: Feed span; A molten steel receiving span is arranged in parallel with the charging span, and at least one baking station is arranged in the molten steel receiving span; A cross-span trolley that can move back and forth between the molten steel receiving span and the charging span; A plurality of ladles and ladles covers, wherein the ladles are arranged in the feeding span; and a baking device and a temperature monitoring device are arranged on the ladles covers.
4. The system according to claim 3, characterized in that: It also includes a cover-adding mechanism, which is arranged in the molten steel receiving span and cooperates with the molten iron ladle.
5. The system according to claim 3, characterized in that: The baking device is a gas baking device, which is provided with a plurality of gas baking burners.
6. The system according to claim 5, characterized in that: The excess air coefficient of the gas baking burner is 0.95-1.
02.
7. The system according to claim 3, characterized in that: The charging span and the molten steel receiving span are both equipped with cranes.
8. The system according to claim 3, characterized in that: Two baking stations are arranged in the molten steel receiving span, or one baking station and one temporary parking station are arranged.
Citation Information
Patent Citations
Method for recycling residual hot steel slag in continuous casted steel ladle
CN102399917A
Method for recycling steel-ladle hot-state casting residues by means of converter
CN109609721A
Method for recovering molten steel of casting residue slag return ladles in hot state
CN110273047A