Method and device for preventing heavy ladle from sticking in casting residue returning production process
By reacting oxygen with molten iron and igniting CO gas to maintain ladle temperature, the method prevents slag sticking, ensuring continuous operation and reducing maintenance costs in steel production.
Patent Information
- Application Number
- CN202310661283.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-06
- Publication Date
- 2024-12-06
AI Technical Summary
The issue of casting slag sticking to the inner wall of the ladle due to temperature drop during the recycling process, leading to operational inefficiencies and increased maintenance costs in steel production.
A method involving the use of oxygen to react with molten iron in the ladle, generating heat through exothermic reactions, and igniting CO gas and O2 to maintain temperature, combined with ladle swinging to promote mixing and heat transfer, preventing slag sticking.
Prevents slag sticking by maintaining ladle temperature, ensuring continuous operation and reducing maintenance costs, thereby enhancing production efficiency and safety.
Smart Images

Figure CN119082384A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of recycling and utilizing steel slag, and in particular to a method and a device for preventing a heavy ladle of molten iron from sticking in a production process in which casting slag is returned. Background Art
[0002] In the long process of steel production, in the blast furnace-converter process, after the molten steel on the continuous casting platform is cast, there will always be a part of the molten steel and hot slag left in the ladle on the platform that cannot be put into the middle ladle. This is to ensure the quality of the subsequent continuous casting billets. The remaining hot melt in the ladle is usually the casting slag in a broad sense.
[0003] The broad sense of the casting slag contains two parts of melt, one is the liquid metal part in the broad sense of the casting slag - that is, molten steel, and the other is the liquid slag part in the broad sense of the casting slag - that is, the narrow sense of the casting slag. Since the density of the molten steel in the broad sense of the casting slag and the narrow sense of the casting slag is quite different, the density of the molten steel is much greater than that of the narrow sense of the casting slag, so usually the bottom of the ladle is molten steel, and the narrow sense of the casting slag is above the molten steel.
[0004] For a 300t converter steel plant, there are usually 6-10t of broad casting slag, of which molten steel and narrow casting slag each account for half, that is, there are 3-5t of molten steel and 3-5t of narrow casting slag in the casting ladle. Because this part of the melt contains valuable refined molten steel and has huge thermal energy, returning the broad casting slag to production can achieve higher productivity, higher production benefits and significant energy-saving and consumption-reducing advantages.
[0005] In the existing generalized casting slag recycling technology, there are several return paths: one is to return to the refining furnace, the second is to return to the converter, and the third is to return to the desulfurization process. Among them, the second and third paths both require pouring the generalized casting slag into the ladle, and then returning the ladle to the process before the converter. This is the generalized casting slag recycling technology.
[0006] Since the return of generalized casting slag is intermittent, the interval period is usually about half an hour. Considering the temperature drop of generalized casting slag, a part of molten iron can be pre-loaded in the ladle first, and then the generalized casting slag can be collected. This ladle with pre-loaded molten iron is called a heavy-bag ladle.
[0007] For 300t converter steel plants, 30t of molten iron is usually pre-loaded in the ladle. With the heat reserve of 30t of molten iron, the ladle can receive generalized casting slag 3 to 5 times. In the interval between each time the ladle receives casting slag, the casting slag in the ladle is open to cool down. In addition, when the generalized casting slag is injected into the ladle, since the narrow casting slag in the generalized casting slag is oxidizing, it will react with the molten iron with reducing elements in the ladle, and the reaction is endothermic. In addition, the heat dissipation during the waiting period for receiving the casting slag causes the temperature of the melt in the ladle to drop, which can easily reduce the temperature of the slag in the ladle to the extent that it adheres to or condenses on the inner wall of the ladle, causing the casting slag in the ladle to stick to the ladle, which has a bad impact on the subsequent ladle pouring and pouring of the melt. The repair of the ladle after slag sticking affects the life of the ladle refractory materials, increases the production and repair costs, and more seriously affects the continuous operation of the casting slag return production process, causing multiple operating losses to the steel mill.
[0008] Therefore, how to prevent the casting slag from sticking to the ladle due to the drop in slag temperature after being poured into the ladle becomes a technical problem that needs to be solved urgently. Summary of the invention
[0009] The purpose of the present invention is to provide a method and device to prevent the casting slag from sticking to the heavy-clad iron ladle during the production process of the casting slag return, solve the problem of the slag sticking to the wall of the iron ladle during the production process of the casting slag return, promote the improvement of the casting slag return production process, and have significant economic and environmental benefits.
[0010] To achieve the above object, the technical solution of the present invention is:
[0011] A method for preventing casting slag from sticking to a heavy-clad iron ladle during a production process, comprising the following steps:
[0012] 1) After the molten iron is filled into the ladle for use, the amount of molten iron filled is 10-15% of the molten iron volume. The ladle filled with molten iron is called a heavy ladle;
[0013] 2) After the molten steel is poured, the casting slag in the ladle is injected into the heavy ladle iron ladle, and during or after the casting slag is poured, oxygen is blown into the melt of the heavy ladle iron ladle, and the oxygen reacts with the molten iron in the ladle until the heavy ladle iron ladle takes on the casting slag again;
[0014] At the same time, the CO gas and O2 escaping from the casting slag are burned by an ignition device above the heavy iron ladle slag layer;
[0015] Repeat the above operation until the heavy ladle completes receiving the casting slag;
[0016] 3) Return the heavy ladle that receives the casting slag to production.
[0017] Preferably, in step 2), oxygen is blown continuously or intermittently into the molten iron in the heavy ladle iron ladle by an oxygen lance through the casting slag layer.
[0018] Preferably, in step 2), during the oxygen blowing process, the position of the oxygen lance is continuously adjusted to ensure that the oxygen is evenly dispersed in the molten iron.
[0019] Preferably, the amount of oxygen required per ton of casting slag is 250-700 L / min, and the oxygen supply pressure is 0.15-0.35 MPa.
[0020] Preferably, the ladle is swung about the center line of its ear axis before the casting slag is poured into the ladle and before it receives the casting slag again.
[0021] Preferably, the unilateral swing angle of the ladle is less than 21°.
[0022] In the method of the present invention:
[0023] In the interval between the heavy ladle receiving the casting slag and the heavy ladle receiving the casting slag again, the oxygen lance is passed through the casting slag layer and inserted into the molten iron layer of the heavy ladle, and oxygen is blown into the molten iron layer continuously or intermittently. The oxygen lance passes through the casting slag part of the upper layer in the ladle and enters the molten iron part of the lower layer. The oxygen reacts with the exothermic elements Si, Mn, C, P, etc. in the molten iron, releases reaction heat, and generates CO gas. The unreacted oxygen and the generated CO gas escape from the melt, and produce a combined stirring effect on the mixed melt of molten iron and casting slag, so that the generated heat can be smoothly transferred to the mixed melt, and the mixed melt of molten iron and casting slag is heated, thereby compensating for the heat absorption in the reaction process between the casting slag and the molten iron.
[0024] When the casting slag is poured into the molten iron ladle, oxygen is blown through an oxygen lance, and the oxygen and the molten iron are partially oxidized to release heat. Due to the momentum impact of the injected casting slag and the stirring effect of the CO gas generated by the partial oxidation and heat release of the molten iron, it will be more conducive to quickly and evenly replenishing heat for the mixed melt of molten iron and casting slag.
[0025] At the same time, an ignition device is arranged above the slag layer to ignite the CO gas and O2 overflowing from the melt below to release heat, so that a mild combustion heat release layer on the upper layer of the molten slag is formed in the ladle, so that the temperature of the exposed furnace lining above the ladle will not drop too much. In addition, the surface casting slag layer of the ladle is radiated by the flame, which compensates for the heat dissipation of the casting slag, and the temperature of the surface casting slag will not drop too much, thus eliminating the concern of slagging of the surface casting slag in the gap receiving the casting slag.
[0026] The double heat release of blowing and baking ensures that the temperature of the casting slag will not drop too much during the production process, and avoids the phenomenon of the casting slag sticking to the inner wall of the ladle and solidifying.
[0027] The casting slag is poured into the ladle and before it receives the casting slag again, the ladle is swung with the center line of its ear axis as the axis, that is, the ladle is placed on a trolley whose body can be swung back and forth with the center line of its ear axis as the axis. This can promote forced convection movement between the casting slag layer and the molten iron layer in the ladle, promote uniform heating of the casting slag and molten iron eutectic by oxidation exothermicity and combustion exothermicity to a greater extent, eliminate the slag ring layer adhered to the ladle wall, prevent the ladle lining from experiencing a large temperature drop, ensure the stable operation of the process and equipment, and promote the optimized operation of the casting slag return production.
[0028] The present invention also provides a device for the method of preventing the heavy iron ladle from sticking during the production process of the casting slag return, which comprises:
[0029] Ladle;
[0030] An oxygen lance, the oxygen lance body of which is inserted into the ladle;
[0031] An ignition device is arranged in the upper part of the ladle.
[0032] Preferably, the ladle is placed on a trolley, a plurality of retractable top rods and support columns are provided at the bottom of the trolley, and a retractable support rod is provided inside the support column.
[0033] Preferably, a dust hood is provided above the ladle.
[0034] The differences and improvements of the present invention over the prior art are as follows:
[0035] Chinese patent CN2018102072178 discloses "a method for recovering molten steel by returning hot casting slag to a ladle", which receives and circulates multiple ladles of casting slag by setting up a heat preservation furnace in the molten steel receiving span. The function of the heat preservation furnace is to heat the casting slag by induction heating or oxygen blowing, and pour at least three ladles of casting slag. Since the casting slag is a poor conductor of heat, no matter whether induction heating or oxygen blowing is used for heating, the thick slag layer cannot be heated, and the slag layer on the upper surface will also cool down and solidify, which cannot play the role of heating or heat preservation of the slag.
[0036] Chinese patent CN2018115574613 discloses "a method for recycling hot casting slag from ladle in converter", step 1): after the converter taps steel, the converter slag is splashed in the converter, and the converter slag is splashed and all of it remains in the converter, located at the bottom and lining of the converter; step 2): the hot metal is desulfurized and pretreated in the molten iron tank, and the hot casting slag is mixed with the molten iron after slagging and added to the converter for converter smelting. After the molten iron is pretreated and slag is removed, the temperature of the molten iron will be greatly reduced, and then the casting slag is directly poured into it. The further reaction of the casting slag and the molten iron will absorb heat, so the casting slag is easy to stick to the ladle. When pouring molten iron to the converter, the slag on the wall of the molten iron ladle will make it difficult to predict the path, direction and speed of the molten iron being poured into the converter. It is very likely that the molten iron and slag will splash everywhere, or even splash out of the converter, which will bring great danger to the operation of adding molten iron to the converter.
[0037] Chinese patent CN2010102764524 discloses "a method for recycling and reusing hot slag from continuous casting ladle". In continuous casting production, after the ladle molten steel is injected into the tundish, the molten hot slag in the ladle is poured into the heavy iron tank; then the hot slag is added to the converter together with the molten iron for steelmaking. The patent mentions that the slag may coagulate, but no solution is proposed. The present invention focuses on how to prevent the casting slag from coagulating due to continuous cooling.
[0038] Chinese patent CN2014102591190 discloses "an operation method for recovering continuous casting excess slag in a molten iron tank". In this patent, a heavy ladle is also used to receive the excess slag. However, the amount of molten iron in the ladle must reach 70-80% of the total amount of molten iron in the ladle at the beginning, while the amount of pre-loaded molten iron in the present invention is only about 10%. Therefore, the present invention has ample space to accept multiple furnaces of superheated molten steel to make up the heat. Therefore, the amount of superheated molten steel poured in can have a relatively large drop and impulse to vigorously stir and turn the shallower molten iron and the excess slag, promote the blending and mixing of the two and facilitate heat transfer. Otherwise, a small amount of superheated molten steel and a small pouring drop cannot cause the liquid in the ladle to tumble violently, and the heat cannot be transferred well.
[0039] Compared with the prior art, the present invention has the following beneficial effects:
[0040] In order to prevent the casting slag from sticking, slagging and sticking in the production process, the prior art mainly focuses on how to quickly return the casting slag to production or improve the equipment.
[0041] The present invention blows oxygen into the melt of the heavy-laden iron ladle, and the oxygen reacts with the molten iron in the ladle, and the reaction between the oxygen and the molten iron is an exothermic reaction, which compensates for the heat absorption in the reaction process of the casting slag and the molten iron; at the same time, above the slag layer of the casting slag, the CO gas and O2 overflowed from the reaction will burn and release heat to compensate for the heat dissipation of the gap between the casting slag, thereby ensuring that the temperature of the casting slag will not drop significantly, and even if multiple packages of casting slag are received, the phenomenon of the casting slag sticking and solidifying on the inner wall of the iron ladle can be avoided, which helps to continuously improve the casting slag recycling production technology, form a good process technology guarantee, and jointly achieve the improvement of the efficiency of the steel plant. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 This is a schematic diagram of a device for Example 1 of the method of the present invention;
[0043] Figure 2 This is a schematic diagram of a device for Example 2 of the method of the present invention;
[0044] Figure 3 This is a schematic diagram of the device of Example 3 of the method described in the present invention. DETAILED DESCRIPTION
[0045] See also Figure 1 to Figure 3 The device for preventing the casting slag from sticking in the heavy ladle iron ladle during the production process of the present invention comprises:
[0046] Hot metal ladle 1;
[0047] Oxygen lance 2, the oxygen lance body of which is inserted into the inside of the molten iron ladle;
[0048] The ignition device 3 is arranged in the upper part of the ladle 1 .
[0049] Preferably, the ladle is placed on a trolley 4, a plurality of retractable top rods 41 and support columns 42 are provided at the bottom of the trolley, and a retractable support rod 43 is provided inside the support column.
[0050] Preferably, a dust hood 5 is provided above the ladle 1 .
[0051] Example 1
[0052] See also Figure 1 A method for preventing casting slag from sticking to a heavy ladle during a production process, comprising the following steps:
[0053] 1) The ladle 1 is filled with molten iron for standby use, wherein the amount of molten iron filled is 10% of the amount of the molten iron contained. The ladle filled with molten iron is called a heavy ladle;
[0054] 2) After the molten steel is poured, the casting slag in the ladle 100 is injected into the heavy ladle iron ladle 1. During the pouring process of the casting slag or after the pouring of the casting slag, oxygen is blown into the molten iron layer of the heavy ladle iron ladle by using the oxygen lance 2. The oxygen blowing duration is 2 to 5 minutes, and then the oxygen is blown again after an interval of 5 to 10 minutes until the heavy ladle iron ladle takes on the casting slag again. During the oxygen blowing process, the position of the oxygen lance 2 in the melt is continuously moved. The oxygen supply required for each ton of casting slag is 500L / min, and the oxygen supply pressure is 0.20MPa.
[0055] At the same time, the CO gas and O2 escaping from the casting slag are burned above the heavy iron ladle slag layer by using the ignition device 3;
[0056] Repeat the above operation until the heavy ladle 1 has completed receiving the casting slag;
[0057] 3) Return the heavy iron ladle 1 after receiving the casting slag to production and utilization.
[0058] Example 2
[0059] See also Figure 2 A method for preventing casting slag from sticking to a heavy ladle during a production process, comprising the following steps:
[0060] 1) The ladle 1 is filled with molten iron for standby use, wherein the amount of molten iron filled is 12% of the amount of the molten iron container. The ladle filled with molten iron is called a heavy ladle;
[0061] 2) After the molten steel is poured, the casting slag in the ladle 100 is injected into the heavy ladle iron ladle 1. During or after the casting slag is poured, oxygen is blown into the molten iron layer of the heavy ladle iron ladle by an oxygen lance 2 until the heavy ladle iron ladle receives the casting slag again; the oxygen supply required for each ton of casting slag is 400L / min, and the oxygen supply pressure is 0.15MPa;
[0062] At the same time, the CO gas and O2 escaping from the casting slag are burned above the heavy iron ladle slag layer by using the ignition device 3;
[0063] Repeat the above operation until the heavy ladle completes receiving the casting slag;
[0064] 3) Return the heavy ladle that receives the casting slag to production.
[0065] Example 3
[0066] See also Figure 3 A method for preventing casting slag from sticking to a heavy ladle during a production process, comprising the following steps:
[0067] 1) The ladle 1 is filled with molten iron for standby use, wherein the amount of molten iron filled is 15% of the amount of the molten iron container. The ladle filled with molten iron is called a heavy ladle;
[0068] 2) After the molten steel is poured, the casting slag in the ladle 100 is injected into the heavy ladle iron ladle 1. During or after the casting slag is poured, oxygen is blown into the molten iron layer of the heavy ladle iron ladle by using the oxygen lance 2 until the heavy ladle iron ladle takes on the casting slag again. During the oxygen blowing process, the position of the oxygen lance in the melt is continuously moved. The oxygen supply required for each ton of casting slag is 250L / min, and the oxygen supply pressure is 0.35MPa.
[0069] At the same time, the CO gas and O2 escaping from the casting slag are burned by an ignition device above the heavy iron ladle slag layer;
[0070] The ladle is placed on the trolley 4 and swings back and forth with the center line of the ladle's trunnion as the axis. Each time it swings in one direction, the single-side swing angle is less than 21°, and then it is returned to the center, and then it swings in the other direction. After each swing is tilted into place, the ladle can be kept in this position for 5 to 25 minutes;
[0071] Repeat the above operation until the heavy ladle 1 has completed receiving the casting slag;
[0072] 3) Return the heavy iron ladle 1 after receiving the casting slag to production and utilization.
Claims
1. A method for preventing casting slag from sticking to a heavy ladle during the production process, characterized in that: The steps include: 1) After the molten iron is filled into the ladle for use, the amount of molten iron filled is 10-15% of the molten iron volume. The ladle filled with molten iron is called a heavy ladle; 2) After the molten steel is poured, the casting slag in the ladle is injected into the heavy ladle iron ladle. During or after the pouring of the casting slag, oxygen is blown into the melt of the heavy ladle iron ladle. The oxygen reacts with the molten iron in the ladle until the heavy ladle iron ladle receives the casting slag again. At the same time, the CO gas and O2 overflowing from the casting slag are burned by an ignition device above the slag layer of the heavy ladle iron ladle. Repeat the above operation until the heavy ladle completes receiving the casting slag; 3) Return the heavy ladle that receives the casting slag to production.
2. The method according to claim 1, characterized in that: In step 2), oxygen is blown continuously or intermittently into the molten iron in the heavy ladle by an oxygen lance through the casting slag layer.
3. The method according to claim 2, characterized in that: In step 2), during the oxygen blowing process, the position of the oxygen lance is continuously adjusted to ensure that the oxygen is evenly dispersed in the molten iron.
4. The method according to claim 1, characterized in that: The amount of oxygen required per ton of casting slag is 250-700 L / min, and the oxygen supply pressure is 0.15-0.35 MPa.
5. The method according to claim 1, characterized in that: The casting slag is poured into the ladle until the ladle is swung around the center axis of the ear shaft before receiving the casting slag again.
6. The method according to claim 5, characterized in that: The unilateral swing angle of the ladle is less than 21°.
7. A device for preventing casting slag from sticking to a heavy ladle during the production process as claimed in any one of claims 1 to 6, characterized in that: include: Ladle; An oxygen lance, the oxygen lance body of which is inserted into the ladle; An ignition device is arranged in the upper part of the ladle.
8. The device according to claim 7, characterized in that: The molten iron ladle is placed on a trolley, a plurality of retractable top rods and support columns are arranged at the bottom of the trolley, and a retractable support rod is arranged inside the support column.