Method for preparing titanium alloy cast ingot by recovering residual titanium
Through the directional sampling and component sequence design of titanium alloy residues, combined with vacuum consumable arc smelting and stirring technology, the problem of insufficient composition uniformity and stability of titanium alloy ingots is solved, and high-quality titanium alloy recycling ingots is achieved , reducing environmental protection and cost pressure.
Patent Information
- Application Number
- CN202411142388.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-20
AI Technical Summary
The poor composition uniformity and insufficient batch composition stability in the existing titanium alloy residue recycling process lead to unstable quality of titanium alloy ingots, and high environmental protection challenges and high costs.
After collecting the same titanium alloy residues for surface cleaning, casting rods are prepared by smelting by electron beam cold bed furnace or plasma beam cold bed furnace, and directional sampling and component testing are carried out. Electrode blocks with special component sequences are designed to be coupled to the casting rod. Vacuum consumable arc melting is performed, combining DC and AC stirring currents to ensure composition uniformity.
It significantly improves the composition uniformity and batch stability of titanium alloy ingots, reduces the unevenness of oxide content, reduces the demand for acid and alkaline washing, and reduces environmental protection pressure and production costs.
Smart Images

Figure CN119082472A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal material processing, and in particular to a method for recovering residual titanium to prepare a titanium alloy ingot with uniform and stable composition. Background Art
[0002] Titanium alloys have excellent properties such as high specific strength, corrosion resistance, high and low temperature resistance, etc., and are widely used in aviation, aerospace, shipbuilding, chemical industry and other fields. Due to the processing characteristics of titanium materials, the final yield rate is generally less than 50%, and a large amount of residual titanium is generated during the entire production process. Therefore, increasing the recycling of titanium alloy residual materials has significant social and economic benefits.
[0003] At present, there are two most mainstream titanium alloy waste recycling processes: ① acid-base washing of block residual titanium alloy and welding into a whole electrode, or degreasing and cleaning of chip residual titanium alloy and crushing, then mixing with sponge titanium master alloy and pressing into electrode block and then welding into a whole electrode, and melting the above electrode twice in a vacuum consumable arc melting furnace to prepare titanium alloy ingot; ② acid-base washing of block residual titanium alloy, or degreasing and cleaning of chip residual titanium alloy and directly pressing into electrode block, and putting the above block (generally, a part of electrode block pressed by sponge titanium and master alloy will be added) into electron beam cooling furnace, plasma beam cooling furnace or vacuum consumable arc condensation furnace to melt into ingot, and then 1-2 vacuum consumable arc melting to prepare the final titanium alloy ingot. The advantage of solution ① is that the equipment is simple and the cost is relatively low; the advantage of solution ② is that due to the existence of cooling bed / condensation shell, the high-density inclusions in residual titanium can be removed by precipitation. Therefore, the adoption of solution ② can eliminate customers' concerns about metallurgical defects of titanium alloy. Generally, titanium alloys have poor machinability and are easily mixed or pierced with high-density inclusions such as broken carbide tools during processing. Such inclusions cannot be removed by vacuum consumable arc melting, and such inclusions will become a major hidden danger in titanium alloy parts. It should be further pointed out that the electron beam cooling furnace in Scheme ② is currently the most mainstream titanium alloy smelting and recycling solution due to its relatively simple equipment structure and high production efficiency; however, the biggest disadvantage of the electron beam cooling furnace is that compared with all other smelting methods, the required vacuum degree is extremely high due to the presence of the electron beam during smelting, resulting in the maximum volatilization of the molten alloy elements, among which elements such as Al can usually volatilize 5-20wt.%, so the element content control in this process is also the most difficult, while the volatilization of commonly used alloy elements in normal smelting processes of other methods is very small (generally <2 wt.%).
[0004] However, both of the above two mainstream methods have the following problems: The composition uniformity within a single batch of ingots is poor, and the composition stability between multiple ingot batches is very poor. This is mainly due to the large amount of residual titanium raw materials required for the smelting of a single ingot, and the composition of a single piece of residual titanium is difficult to grasp. Therefore, it is impossible to accurately design the composition of the entire ingot, resulting in very poor composition stability in multiple batches, and it is also difficult to uniformly design the distribution of different smelting parts of a single ingot, resulting in poor composition uniformity of a single ingot. There are two main reasons for this: First, residual titanium mainly comes from the riser, bottom plate, surface chips of titanium alloy ingots, the head, bottom, corners of bars and forgings, etc., and its composition is very different from the mother ingot from which it comes, and its own composition fluctuations in different regions are also very large, making it difficult to conduct composition tests in each or everywhere to grasp its true composition status; second, residual titanium can come from different ingot numbers, or even materials from different manufacturers, but residual titanium is generally large in number but small in size, making it difficult to trace and manage, so it is difficult to know its true composition through tracing, and because of the huge quantity, it is difficult to know its true composition status through chemical composition testing. In addition, if the electron beam cold bed melting and recycling route is adopted, the extremely high vacuum in the electron beam melting environment leads to high volatility of the melting elements, which exacerbates the difficulty of composition control; As the main source of waste, bulk waste is overly dependent on alkaline pickling. In addition to oil stains, the surface of bulk residual titanium generally contains surface oxides. It is usually necessary to pickle and alkali wash the residual titanium for surface treatment. Otherwise, it is impossible to know the oxygen content brought by the residual titanium oxide to the recycled ingot, which may cause the oxygen content of the ingot to exceed the range specified in the national standard GB3620.1 or the range expected by the customer (Note: Oxygen itself is an alloying element of titanium alloy. Generally, the oxygen content of titanium alloy has a range. Too high and too low are not in compliance with the standard). However, acid and alkali washing will bring environmental challenges. The relevant investment is usually difficult to pass the environmental impact assessment and the equipment system investment is large, which hinders the treatment of residual titanium and then hinders the recycling of titanium alloys. In fact, since the oxygen content of sponge titanium is very low, it can usually reach ≤0.04 wt.%, while the oxygen content required for titanium alloy ingots is generally 0.10-0. 20 wt.%, in the process of producing titanium alloys, TiO2 oxide is added as raw material. Therefore, relative to the bulk matrix, a relatively thin layer of surface oxide formed on the surface of the titanium alloy during the hot working process actually has a low total oxygen content in the material and has the potential to be added as a raw material to the alloy ingot.
[0005] Therefore, the current commonly used methods for the recovery of residual titanium are not only environmentally challenging, but also Since the raw material composition cannot be fully understood during each smelting, or the smelting process is difficult to control (if electron beam cold bed smelting is used), this production method with poor composition uniformity and poor batch composition stability has seriously aggravated customers' concerns about the quality of titanium alloy recycling products, reduced the value of residual titanium recycling, and significantly hindered the development of the residual titanium recycling business. Summary of the invention
[0006] In view of the problems existing in the above-mentioned prior art in recycling and remelting titanium alloys, the purpose of the present invention is to provide a method for recycling residual titanium to prepare titanium alloy ingots, which is not only environmentally friendly but also can prepare titanium alloy ingots with uniform and stable composition.
[0007] To achieve the above purpose, the technical solution adopted by the present invention is as follows: A method for recovering residual titanium to prepare a titanium alloy ingot, characterized in that it comprises the following steps: Step 1), collecting titanium alloy residues of the same grade and cleaning the surface of the residual titanium; Step 2), using an electron beam cooling furnace or a plasma beam cooling furnace or a vacuum consumable arc shell furnace to melt the residual titanium in step 1), and then solidify it into a round titanium alloy casting rod; Step 3), sampling the titanium alloy cast rod obtained in step 2) at a position within 300 mm from the head end face and the bottom end face in the longitudinal direction, sampling at intervals of 200-1000 mm from the remaining parts of the titanium alloy cast rod, and then testing the composition of the sampled samples, and obtaining the composition distribution of the entire titanium alloy cast rod in the longitudinal direction by linear interpolation; Step 4), weigh, mix and press the titanium sponge and the intermediate alloy into an electrode block with a circular center hole according to a specially designed component sequence, then stack and weld the electrode blocks in order, insert the titanium alloy cast rod obtained in step 2) into the circular center hole of the electrode block in a preset head-bottom direction before or after welding to form a coaxial composite electrode; then load the composite electrode into a vacuum consumable arc melting furnace, use the same brand of auxiliary electrode to weld and fix the composite electrode, perform the first vacuum consumable arc melting, and use a DC stirring current during the melting; then turn the composite electrode around for a second vacuum consumable arc melting, and use an AC stirring current during the melting, and finally obtain a titanium alloy ingot; wherein, the specially designed component sequence needs to meet the following requirements: in the longitudinal direction of the composite electrode, with the length of a single electrode block as a unit, the composition of the titanium alloy cast rod portion corresponding to each unit and the composition of the electrode block should be weighted averaged to obtain the composition of each unit, and the composition of all units should be consistent. That is, the average composition C of the entire composite electrode = the average composition C of any unit i = (Any electrode block component C block-i ×Weight of any electrode block mblock-i+ The component C of the cast rod part to which this unit corresponds bar-i ×The weight of the cast rod m bar-i ) / (weight of any electrode block m block-i +The weight of the cast rod corresponding to this unit m bar-i ).
[0008] Further, the length of a single electrode block (ie, the length in the longitudinal direction of the composite electrode) is 200-600 mm.
[0009] Furthermore, in the first vacuum consumable arc melting, the setting value of the DC stirring current is determined by the stirring magnetic field strength it generates, which is 4-6mT; the AC stirring magnetic field strength during the second vacuum consumable arc melting is 1-3mT and the stirring period is 4-12s.
[0010] Furthermore, the shape of the electrode block is circular or regular octagonal.
[0011] Furthermore, the surface cleaning in the above step 1) is specifically performed by using a conventional environmentally friendly degreasing solvent and water to clean the surface in sequence.
[0012] Furthermore, the diameter of the center hole of the electrode block is 110-640 mm; and when producing the same ingot, the diameter of the cast rod used is 10-40 mm smaller than the diameter of the center hole of the electrode block, and the difference between the length of the cast rod and the total length of the electrode block is ≤10 mm. When the diameter of the cast rod is 10-20 mm smaller than the diameter of the center hole of the electrode block, it is inserted into the center hole before the electrode block is welded, and when the former diameter is 20-40 mm smaller than the latter diameter, the cast rod is inserted into the center hole after the electrode block is welded.
[0013] Furthermore, the length of the cast rod is 2000-6000 mm, and the difference between the length of the cast rod and the total length of the electrode block is ≤10 mm.
[0014] Furthermore, the outer diameter (outer circle diameter or circumscribed circle diameter) of the electrode block is 420-880 mm, and the pressing density of the electrode block is 3.2-3.6 g / cm 3 .
[0015] Furthermore, in the above composite electrode, the weight of the cast rod accounts for 8-60 wt.% of the weight of the entire composite electrode.
[0016] Furthermore, the titanium content in the titanium alloy residue (i.e., residual titanium) in the above step 1) is ≥ 70 wt.%.
[0017] Furthermore, in the above step 2), the power of a single electron gun in the electron beam cold hearth melting furnace is 300-500 kW; the power of a single plasma gun in the plasma beam cold hearth melting furnace is 300-800 kW; the melting current / voltage of the vacuum consumable arc shell furnace is set at 25-55 kA / 25-40V, and the same brand of consumable electrodes with a composition close to the target are used during melting.
[0018] Furthermore, the diameter of the auxiliary electrode used in the first vacuum consumable arc melting is larger than the diameter of the cast rod and smaller than the outer diameter of the composite electrode.
[0019] Furthermore, the melting current / voltage is 12-20 kA / 22-28 V during the first vacuum consumable arc melting; and the melting current / voltage is 15-30 kA / 24-35 V during the second vacuum consumable arc melting.
[0020] Furthermore, the diameter of the crucible used in the first vacuum consumable arc melting is 520-980 mm, and the diameter of the crucible used in the second vacuum consumable arc melting is 600-1080 mm.
[0021] Furthermore, the diameter of the titanium alloy ingot after two vacuum consumable arc melting is 600-1080 mm and the weight is 2000-12000 Kg.
[0022] Compared with the prior art, the present invention has the following beneficial effects: 1. Due to the large number of residual titanium alloy blocks and scraps, the uncertainty of the components of each unit, and the difficulty of process control, it is difficult to prepare high-quality titanium alloy recycling ingots with uniform and stable components. However, this application will carry out directional sampling of the cast bars that have been initially smelted in a cooling furnace or a solidification furnace, test the sample composition, and then prepare an electrode block with a circular center hole according to the requirements of a specially designed component sequence, and finally coaxially couple the electrode block with the cast bar, which can bring the following main benefits: ① Recycling cast rods with uneven composition in the longitudinal direction, adjusting the composition of the electrode block, so that the entire composite electrode has uniform composition in the longitudinal direction, and then preparing titanium alloy ingots with more uniform overall composition, thereby improving the uniformity of the composition of a single titanium alloy ingot. It should be noted here that during vacuum consumable arc melting, the molten pool is raised and solidified layer by layer. In short, when melting to the head, the bottom has already solidified. Therefore, if the present invention is not adopted, it is difficult to eliminate the composition differences in the longitudinal direction of the ingot that are prone to exist in the cold bed furnace melting through multiple vacuum consumable arc melting; ② Each time an ingot is produced, the ingredients added can be accurately controlled. This not only enables better control of the target composition of a single ingot, but also greatly improves the composition stability between batches of multiple ingots because each ingot is in a controlled state; ③ Since the composition of the ingot after smelting in the cooling hearth furnace or the solidification shell furnace can be tested, the oxide scale on the surface no longer needs to be removed by acid and alkali washing, which not only reduces the processing cost but also reduces the pressure on environmental protection. In the high temperature environment of the cooling hearth / solidification shell smelting, titanium oxide will decompose and melt into the molten pool again, and because the size of oxygen atoms is extremely small, it can be quickly diffused and evenly distributed in the molten pool as a solid solution oxygen element; ④In the coupling design, the cast rod is inserted into the central hole of the electrode block, and the cast rod is circular, and the electrode block is circular or nearly circular (regular octagonal) in design, which can ensure the overall composition consistency of the composite electrode in the longitudinal direction; 2. Due to the inhomogeneity of the residual titanium component, the composition of the cast rod is not only inhomogeneous in the longitudinal direction, but also in the transverse direction. The present application further ingeniously utilizes the horizontal stirring characteristics of the vacuum consumable arc melting furnace itself (the main function of the vertical magnetic field generated by the stirring design of the vacuum consumable arc melting furnace equipment itself is to cause the molten pool to rotate on the horizontal plane). During the first smelting process, a DC stirring magnetic field with a certain strength is applied to make the molten pool rotate at high speed on the horizontal plane, so that the molten droplets with certain differences in composition generated by the synchronously smelted electrode blocks and cast rods can be fully and evenly mixed in the molten pool after dripping into the molten pool, thereby preparing a titanium alloy ingot with uniform composition in both the longitudinal and transverse directions. If other non-center hole structural designs are used, or a DC stirring magnetic field with a certain strength is not used, it is difficult to ensure uniform mixing. At the same time, when coaxially coupled, the use of a double circular or nearly circular composite electrode structure is more advantageous, which is conducive to the homogeneous distribution of components on the circumference and the stable and uniform mixing of the molten pool during smelting. If a square or other design with lower roundness is used, the overall stability of the molten pool will deteriorate, resulting in a weakened uniformity of components. In addition, in the subsequent second vacuum consumable arc smelting, the present invention uses an AC stirring current to obtain a relatively stable molten pool, the main purpose of which is to obtain a stable solidification structure and a smaller macro-micro segregation (so generally cannot be strongly stirred), thereby obtaining a high-quality titanium alloy ingot. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 Schematic diagrams of cross-section and longitudinal section of the composite electrode after assembly according to the present invention, wherein (a) is a schematic diagram of cross-section and (b) is a schematic diagram of longitudinal section. DETAILED DESCRIPTION
[0024] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. It should be understood that the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.
[0025] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.
[0026] The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention. The following specific examples are provided to describe the method of the present application, and other preparation parameters not mentioned in each example are kept consistent in all examples.
[0027] Example 1 (TC4 alloy recovery ingot with a diameter of Φ880 mm and a nominal composition of Ti-6.0Al-4.0V-0.18O) The TC4 titanium alloy block residues were collected, and the surface of the residual titanium was cleaned in sequence with conventional environmentally friendly oil removal solvents and water. After drying, they were placed in the electron beam cooling bed charge box, and three electron guns with a single electron gun power of 350 kW were used for sweeping, cooling bed melting and crystallization melting, respectively, to prepare round titanium alloy cast rods with a diameter of 350 mm and a length of 4800 mm. The cast rods were sampled and tested every 400 mm from the head to the bottom, and the sampled test components were added at 200 mm from the head end face and 200 mm from the bottom end face. The composition distribution in the longitudinal direction of the cast rod was calculated by linear interpolation. The composition sequence of the electrode block was designed according to the composition distribution, so that the composition of the composite electrode after composite in the longitudinal direction was consistent with the nominal composition. A mixing machine was used to automatically mix the materials one by one. A 1 / 2 circle electrode block with a pressing length (axial length of the electrode) of 400 mm was pressed, and the number of electrode blocks was 24. The outer diameter of the electrode block was 680 mm, and the diameter of the center hole was 360 mm. mm, the weight of a single electrode block is 173 kg, and the pressing density of the electrode block is 3.3 g / cm 3; Stack and compact the electrode blocks in order (two 1 / 2 circle electrode blocks in each layer are combined into one electrode block), and insert the titanium alloy cast rod with a preset head-bottom direction into the center hole to make it a composite electrode, and use a vacuum plasma welding box to weld it into a welding electrode; load the composite electrode into a vacuum consumable arc melting furnace; place an auxiliary electrode of the same grade with a diameter of Φ400 mm and similar composition at the head of the vertical composite electrode, and start arc welding between the auxiliary electrode and the composite electrode so that the two components of the composite electrode are welded and fixed to the auxiliary electrode, and then carry out the first vacuum consumable arc melting, the crucible diameter of the first melting is 780 mm, the melting current / voltage is 15kA / 23V, and the DC stirring magnetic field strength is set to 5.0 mT during melting (the stirring current of a certain type of ALD vacuum consumable arc melting furnace used in the corresponding experiment is set to 20A); then carry out the second vacuum consumable arc melting, the melting crucible diameter is 880 mm, the melting current / voltage was 22kA / 28V, and the AC stirring magnetic field intensity / cycle was set to 2.5mT / 10S during melting (the corresponding stirring current was set to 10A), and finally a titanium alloy ingot was obtained.
[0028] The titanium alloy ingots were sampled at 5 positions, namely the head (200 mm from the head end), 1 / 4, middle, 3 / 4 and bottom (200 mm from the bottom end), and 4 samples were taken at 90° intervals on the circumference of each position, for a total of 20 samples for chemical composition testing. At the same time, 10 batches were produced continuously using the same method. Finally, the test data results of all ingots showed that the elemental composition of the ingots met the requirements of the national standard GB3620.1, the main Al, V and O elements fluctuated around the nominal composition, and the maximum difference of Al element in the same ingot of all ingots was 1200ppm, and the maximum difference between ingots was 1900ppm; the maximum difference of V element in the same ingot was 900ppm, and the maximum difference between ingots was 1500ppm; the maximum difference of O element in the same ingot was 80ppm, and the maximum difference between ingots was 150ppm.
[0029] Example 2 (TC18 alloy recovery ingot with a diameter of Φ680 mm and a nominal composition of Ti-5.0Al-5.0Mo-5.0V-1.0Cr-1.0Fe-0.12O) The TC18 titanium alloy block residues were collected, and the surface of the residual titanium was cleaned with conventional environmentally friendly oil removal solvents and water in turn. After drying, they were placed in the melting crucible of a vacuum consumable shell furnace. Consumable electrodes of the same brand with a similar target composition were used during the smelting. The smelting current / voltage was 40kA / 35V. After the smelting was completed, the melt was poured into a crystallizer to prepare cast rods with a diameter of 250 mm and a length of 4000 mm. The composition of the cast rod was tested every 500 mm from the head to the bottom, and additional sampling and testing were carried out at 250 mm from the end face of the head of the cast rod and 250 mm from the end face of the bottom of the cast rod. The composition distribution of the cast rod was calculated by linear interpolation. The composition sequence of the electrode block was designed according to the distribution so that the composition of the composite electrode in the longitudinal direction was consistent with the nominal composition. A mixing machine was used to automatically mix the materials piece by piece, and a 1 / 2 circle electrode block with a pressing length (axial length of the electrode) of 400 mm was pressed. The number of electrode blocks was 20, the outer diameter of the electrode block was 480 mm, the diameter of the center hole was 280 mm, the weight of a single electrode block was 81 kg, and the pressing density of the electrode block was 3.4 g / cm 3 ; Stack the electrode blocks in order and press them tightly, and weld them in a vacuum plasma welding box to make welding electrodes; load the electrodes into a vacuum consumable arc melting furnace, insert the cast rod into the center hole in a preset head-bottom direction to make it a composite electrode, place a Φ350 mm diameter auxiliary electrode of the same brand with similar components at the head of the vertical composite electrode, and start arc welding between the auxiliary electrode and the composite electrode so that both components of the composite electrode are welded and fixed to the auxiliary electrode; perform the first vacuum consumable arc melting, the melting crucible diameter is 580 mm, the melting current / voltage is 17 kA / 25 V, and the DC stirring magnetic field strength is set to 4.5 mT during the melting (the stirring current of a certain type of ALD vacuum consumable arc melting furnace used in the corresponding experiment is set to 18 A); then perform the second vacuum consumable arc melting, the melting crucible diameter is 680 mm, the melting current / voltage was 24kA / 28V, and the AC stirring magnetic field intensity / cycle was set to 2.0mT / 6S (the stirring current was set to 8A) during the melting, and finally a titanium alloy ingot was obtained.
[0030] The ingot was sampled at 5 positions, namely the head (200 mm from the head end), 1 / 4, middle, 3 / 4 and bottom (200 mm from the bottom end), and 4 samples were taken at 90° intervals on the circumference of each position, for a total of 20 samples for chemical composition testing. At the same time, 10 batches were produced continuously using the same method. Finally, the test data results of all ingots showed that the elemental composition of the ingots met the requirements of the national standard GB3620.1, and the main Al, Mo, V, Cr, Fe, and O elements fluctuated around the nominal composition, and the maximum difference of Al element in the same ingot of all ingots was 1200ppm, and the maximum difference between ingots was 1900ppm; the maximum difference of Mo element in the same ingot was 1500ppm, and the maximum difference between ingots was 1800ppm; the maximum difference of V element in the same ingot was 1200ppm, and the maximum difference between ingots was 1600ppm; the maximum difference of Cr element in the same ingot was 400ppm, and the maximum difference between ingots was 900ppm; the maximum difference of Fe element in the same ingot was 500ppm, and the maximum difference between ingots was 1100ppm; the maximum difference of O element in the same ingot was 70ppm, and the maximum difference between ingots was 130ppm.
[0031] Example 3 (TA15 alloy recovery ingot with a diameter of Φ780 mm and a nominal composition of Ti-6.5Al-1.0Mo-1.0V-2.0Zr-0.13O) The TA15 titanium alloy block residues were collected, and the surface of the residual titanium was cleaned in sequence with conventional environmentally friendly oil removal solvents and water. After drying, they were placed in the electron beam cooling bed charge box, and three electron guns with a single electron beam power of 350 kW were used for sweeping, cooling bed melting and crystallization melting to prepare titanium alloy cast rods with a diameter of Φ350 mm and a length of 4800 mm. The cast rods were sampled and tested every 400 mm from the head to the bottom, and additional sampling and testing were performed at 200 mm from the end face of the head of the cast rod and 200 mm from the bottom end face of the cast rod. The composition distribution of the titanium alloy cast rods was obtained by linear interpolation. The composition sequence of the electrode block was designed according to the distribution so that the composition of the composite electrode in the longitudinal direction was consistent with the nominal composition. A mixing machine was used to automatically mix the materials one by one. A 1 / 2 regular octagonal electrode block with a pressing length (axial length of the electrode) of 400 mm was pressed. The number of electrode blocks was 24, and the diameter of the circumscribed circle of the electrode block was 580 mm and the diameter of the center hole was 360 mm. mm, the weight of a single electrode block is 103 kg, and the pressing density of the electrode block is 3.5 g / cm 3; Stack the electrode blocks in order and compact them, insert the titanium alloy cast rod with a preset head-bottom direction into the center hole to make it a composite electrode, and use a vacuum plasma welding box to weld it to make it a welding electrode; load the electrode into a vacuum consumable arc melting furnace; place an auxiliary electrode of the same brand with a diameter of Φ400mm and similar composition at the head of the vertical composite electrode, and start arc welding between the auxiliary electrode and the composite electrode so that the two components of the composite electrode are welded and fixed to the auxiliary electrode, and then carry out the first vacuum consumable arc melting, the diameter of the melting crucible is 680mm, the melting current / voltage is 18kA / 25V, and the DC stirring magnetic field intensity is set to 5.0 mT during the melting (the stirring current of a certain type of ALD vacuum consumable arc melting furnace used in the corresponding experiment is set to 20 A); then carry out the second vacuum consumable arc melting, the diameter of the melting crucible is 780 mm, the melting current / voltage was 24kA / 27V, and the AC stirring magnetic field intensity / cycle was set to 2.5mT / 10S during melting (the corresponding stirring current was set to 10A), and finally a titanium alloy ingot was obtained.
[0032] The titanium alloy ingots were sampled at 5 positions, namely the head (200 mm from the head end), 1 / 4, middle, 3 / 4 and bottom (200 mm from the bottom end), and 4 samples were taken at 90° intervals on the circumference of each position, for a total of 20 samples for chemical composition testing. At the same time, 10 batches were continuously produced using the same method. Finally, the test data results of all ingots showed that the elemental composition of the ingots met the requirements of the national standard GB3620.1, the main Al, Mo, V, Zr, and O elements all fluctuated around the nominal composition, and the maximum difference of Al element in the same ingot of all ingots was 1300ppm, and the maximum difference between ingots was 2000ppm; the maximum difference of Mo element in the same ingot was 800ppm, and the maximum difference between ingots was 1100ppm; the maximum difference of V element in the same ingot was 700ppm, and the maximum difference between ingots was 1000ppm; the maximum difference of Zr element in the same ingot was 1100ppm, and the maximum difference between ingots was 1600ppm; the maximum difference of O element in the same ingot was 80ppm, and the maximum difference between ingots was 140ppm.
[0033] Comparative Example 1 Except for the following differences, the rest is the same as the first embodiment: Provide residual titanium and pressed electrode blocks of the same weight and source as in Example 1 and place them evenly in the electron beam cooling hearth furnace silo, add a small amount of material close to the target composition as the bottom material of the cooling hearth furnace, and then perform electron beam cooling hearth melting to directly prepare cast rods with a diameter of Φ680 mm. Among them, the principle of the composition design of the electrode block is: estimate the content of each element in the residual titanium, estimate the volatilization amount of each element in the electron beam melting based on experience (the volatilization loss of Al here is estimated to be 10 wt.%, and the volatilization loss of V is estimated to be 4 wt.%), and design the composition of the electrode block based on these two and the nominal composition of the target. The cast rod is directly melted twice in a vacuum consumable arc melting furnace. At the same time, 10 batches are continuously produced using the same method. Finally, the test data results of all ingots showed that the elemental composition of the ingots met the requirements of the national standard GB3620.1, the main Al, V, and O elements fluctuated around the nominal composition, and the maximum difference of Al element in the same ingot of all ingots was 2500ppm, and the maximum difference between ingots was 5600ppm; the maximum difference of V element in the same ingot was 1900ppm, and the maximum difference between ingots was 3800ppm; the maximum difference of O element in the same ingot was 180ppm, and the maximum difference between ingots was 560ppm.
[0034] Comparative Example 2 Except for the following differences, the rest is the same as the second embodiment: The vacuum consumable arc condensation furnace is directly provided with residual titanium and pressed electrode blocks of the same weight and source as those in Example 2, which are evenly placed in the melting crucible of the condensation furnace, and smelted and cast to prepare a cast rod with a diameter of Φ480 mm. Among them, the composition of the electrode block is consistent and the composition design method is: the content of each element in the residual titanium is estimated, and the composition of the electrode block is designed in combination with the nominal composition of the target ingot. The prepared cast rod is directly smelted twice in the vacuum consumable arc smelting furnace. At the same time, 10 batches are continuously produced using the same method. Finally, the test data results of all ingots showed that the elemental composition of the ingots met the requirements of the national standard GB3620.1, and the main Al, Mo, V, Cr, Fe, and O elements all fluctuated around the nominal composition, and the maximum difference of Al element in the same ingot of all ingots was 1900ppm, and the maximum difference between ingots was 4300ppm; the maximum difference of Mo element in the same ingot was 2100ppm, and the maximum difference between ingots was 3600ppm; the maximum difference of V element in the same ingot was 1900ppm, and the maximum difference between ingots was 3700ppm; the maximum difference of Cr element in the same ingot was 900ppm, and the maximum difference between ingots was 2400ppm; the maximum difference of Fe element in the same ingot was 1000ppm, and the maximum difference between ingots was 2600ppm; the maximum difference of O element in the same ingot was 110ppm, and the maximum difference between ingots was 450ppm.
[0035] Comparative Example 3 Except for the following differences, the rest is the same as the third embodiment: The shape of the pressed electrode block is an inner circle and an outer square, and the outer edge is 1 / 2 of a regular quadrilateral. The test results of the final ingot composition are as follows: the maximum difference of Al element in the same ingot is 1600ppm, and the maximum difference between ingots is 2500ppm; the maximum difference of Mo element in the same ingot is 900ppm, and the maximum difference between ingots is 1500ppm; the maximum difference of V element in the same ingot is 1000ppm, and the maximum difference between ingots is 1800ppm; the maximum difference of Zr element in the same ingot is 1300ppm, and the maximum difference between ingots is 1900ppm; the maximum difference of O element in the same ingot is 90ppm, and the maximum difference between ingots is 200ppm.
[0036] Comparative Example 4 Except for the following differences, the rest is the same as the first embodiment: The shape of the pressed electrode block is an inner circle and an outer square, with the outer edge being 1 / 2 of a regular octagon. The test results of the final ingot composition are as follows: the maximum difference of Al element in the same ingot is 1300ppm, and the maximum difference between ingots is 2100ppm; the maximum difference of V element in the same ingot is 1100ppm, and the maximum difference between ingots is 1600ppm; the maximum difference of O element in the same ingot is 90ppm, and the maximum difference between ingots is 150ppm.
[0037] Comparative Example 5 Except for the following differences, the rest is the same as the first embodiment: After multi-point sampling of the cast rod, the average composition of the cast rod is obtained by averaging method instead of linear interpolation method, and the electrode blocks with uniform composition are configured according to the average composition. The test results of the composition of the final produced ingot are: the maximum difference of Al element in the same ingot is 3100ppm, and the maximum difference between ingots is 5200ppm; the maximum difference of V element in the same ingot is 2500ppm, and the maximum difference between ingots is 3800ppm; the maximum difference of O element in the same ingot is 240ppm, and the maximum difference between ingots is 460ppm.
[0038] Comparative Example 6 Except for the following differences, the rest is the same as the first embodiment: The assembly coupling of titanium casting rod and electrode block does not adopt the method of coaxial center hole, but the electrode block is pressed into a structure with a semicircular groove with a diameter of 360 mm on the surface, and the casting rod is placed in the groove, and the two form an eccentric coupling structure. The test results of the composition of the final ingot production are: the maximum difference of Al element in the same ingot is 2100ppm, and the maximum difference between ingots is 2500ppm; the maximum difference of V element in the same ingot is 1800ppm, and the maximum difference between ingots is 2500ppm; the maximum difference of O element in the same ingot is 160ppm, and the maximum difference between ingots is 230ppm.
[0039] Comparative Example 7 Except for the following differences, the rest is the same as the first embodiment: The DC stirring magnetic field strength set during the first vacuum consumable arc melting was 2.0 mT (the corresponding stirring current was set to 8 A). The test results of the final ingot composition were as follows: the maximum difference of Al element in the same ingot was 1900ppm, and the maximum difference between ingots was 2400ppm; the maximum difference of V element in the same ingot was 1500ppm, and the maximum difference between ingots was 1800ppm; the maximum difference of O element in the same ingot was 120ppm, and the maximum difference between ingots was 180ppm.
[0040] Comparative Example 8 Except for the following differences, the rest is the same as the first embodiment: The collected residual titanium was washed with acid and alkali. The test results of the final ingot composition are as follows: the maximum difference of Al element in the same ingot is 1300ppm, and the maximum difference between ingots is 1800ppm; the maximum difference of V element in the same ingot is 900ppm, and the maximum difference between ingots is 1500ppm; the maximum difference of O element in the same ingot is 70ppm, and the maximum difference between ingots is 140ppm.
[0041] Comparative Example 9 Except for the following differences, the rest is the same as Comparative Example 1: The collected residual titanium was washed with acid and alkali. The test results of the final ingot composition are as follows: the maximum difference of Al element in the same ingot is 2600ppm, and the maximum difference between ingots is 5500ppm; the maximum difference of V element in the same ingot is 1800ppm, and the maximum difference between ingots is 3800ppm; the maximum difference of O element in the same ingot is 150ppm, and the maximum difference between ingots is 440ppm.
[0042] It can be seen from Example 1 and Comparative Example 1, and Example 2 and Comparative Example 2 that the use of this technical route can significantly reduce the difference in ingot composition, especially the difference between ingots. That is, this technical route can significantly improve the uniformity and stability of ingot composition.
[0043] It can be seen from Example 1 and Comparative Example 4, and Example 3 and Comparative Example 3 that whether the pressed electrode block is circular or nearly circular also has a certain influence. In the process of industrial production of pressed electrodes, the more common electrode block shapes are not only circular, but also (near) octagonal and (near) quadrilateral. Therefore, the present invention designs three types of circular, regular octagonal and regular quadrilateral for comparative research based on common industrial scenarios. The results show that the closer the shape is to a circle, the better the homogenization effect is, and the more it deviates from a circle, the worse the uniformity of the ingot is. Therefore, this application preferably uses a circle or a regular octagon that is closest to a circle. Although other nearly circular shapes, such as a regular dodecagon, or approximate shapes, such as a slight chamfering improvement on a regular octagon, have not been exhausted one by one, these should all be considered to fall within the scope of protection of this application.
[0044] It can be seen from Example 1 and Comparative Example 5 that if linear interpolation is not used and the composition of the recycled cast rods prepared is assumed to be uniform, it will deviate significantly from the actual situation, resulting in a significant increase in the same-ingot difference of the elements of the ingots finally produced, and a corresponding increase in the difference between ingots.
[0045] From the comparison between Example 1 and Comparative Example 6, it can be seen that the design of the composite structure has an impact on the uniformity of the composition. Among them, whether to assemble the coupling in the form of coaxial center holes has a great impact on the uniformity of the composition. If the coaxial center hole assembly is not adopted, the ingot itself is difficult to homogenize, resulting in a significant increase in the elemental homogeneity of the ingot. Therefore, the assembly of non-coaxial center holes should not be adopted.
[0046] By comparing Example 1 with Comparative Example 7, it can be seen that after the coaxial center hole is assembled, the DC stirring magnetic field intensity of the first vacuum consumable arc melting also has a certain influence on the uniformity of the components. Only with sufficient stirring on the horizontal plane can the composite structure obtain a better mixing effect during melting. Of course, the magnetic field intensity cannot be increased blindly, because under this size condition, excessive stirring will make the melting process unstable. Therefore, there is an upper limit for the optimization of the setting value.
[0047] From the comparison between Example 1 and Comparative Example 8, and Comparative Example 1 and Comparative Example 9, it can be seen that the acid-base washing treatment of residual titanium has a significant impact on the batch stability of the O element ingots recovered by the traditional route (because the whole ingot allocation value of the O element can be more accurately estimated after acid-base washing), and has little effect on the composition uniformity and stability control (especially the O element) of the ingots produced by this technical route. Even without acid-base washing, this technical route can still achieve the uniformity and stability of the O element in the ingots that are significantly better than the traditional route. Therefore, from the perspective of cost and process, the residual titanium recovered under this technical route generally does not need to be washed with acid and alkali. Of course, if the customer has special requirements, for example, the oxygen content of the recovered ingots produced is required to be as low as possible, then the blocky residual titanium can also be acid-base washed and then the ingots can be continued to be produced using this technical route.
[0048] From all the above cases, it can be seen that by exploring the composition of the recovered ingots from the cooling hearth furnace or the solidification furnace, and then adjusting and matching the composition of the electrode block, and then performing vacuum consumable arc melting to prepare the titanium alloy recovered ingots, it has a significant effect on improving product quality, and can improve the uniformity of the ingot composition, especially the stability of the composition of batch ingots. This process uses the cooling hearth furnace or solidification furnace process to process the recovered materials, has no risk of metallurgical defects, has a uniform and stable composition, and has great market value.
[0049] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0050] The above-described embodiments only express several implementation methods of the present application, which is convenient for understanding the technical solution of the present application in detail, but it cannot be understood as limiting the scope of protection of the invention patent. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present application, several modifications and improvements can be made, which all belong to the protection scope of the present application. It should be understood that the technical solutions obtained by those skilled in the art through logical analysis, reasoning or limited experiments on the basis of the technical solutions provided in the present application are all within the protection scope of the claims attached to the present application. Therefore, the protection scope of the patent of this application shall be based on the contents of the attached claims, and the description and drawings can be used to explain the contents of the claims.
Claims
1. A method for recovering residual titanium to prepare titanium alloy ingots, characterized in that: The steps include: Step 1), collecting titanium alloy residues of the same grade and cleaning the surface of the residual titanium; Step 2), using an electron beam cooling furnace or a plasma beam cooling furnace or a vacuum consumable arc shell furnace to melt the residual titanium in step 1), and then solidify it into a round titanium alloy casting rod; Step 3), sampling the titanium alloy cast rod obtained in step 2) at a position within 300 mm from the head end face and the bottom end face in the longitudinal direction, sampling at intervals of 200-1000 mm from the remaining parts of the titanium alloy cast rod, and then testing the composition of the sampled samples, and obtaining the composition distribution of the entire titanium alloy cast rod in the longitudinal direction by linear interpolation; Step 4), the titanium sponge and the intermediate alloy are weighed, mixed and pressed into an electrode block with a circular center hole according to a specially designed component sequence, and then the electrode blocks are stacked and welded in order, and the titanium alloy cast rod obtained in step 2) is inserted into the circular center hole of the electrode block in a preset head-bottom direction before or after welding to form a coaxial composite electrode; then the composite electrode is loaded into a vacuum consumable arc melting furnace, and the composite electrode is welded and fixed with an auxiliary electrode of the same brand, and the first vacuum consumable arc melting is performed, and a DC stirring current is used during the melting; then the composite electrode is turned around for a second vacuum consumable arc melting, and an AC stirring current is used during the melting, and finally a titanium alloy ingot is obtained; wherein the specially designed component sequence needs to satisfy: in the longitudinal direction of the composite electrode, the length of a single electrode block is taken as a unit, and the average value obtained by weighted averaging the composition of the titanium alloy cast rod portion corresponding to each unit and the composition of the electrode block should be consistent among all units, that is, the average composition C of the entire composite electrode = the average composition C of any unit i = (Any electrode block component C block-i ×Weight of any electrode block mblock-i + The component C of the cast rod part to which this unit corresponds bar-i ×The weight of the cast rod m bar-i ) / (weight of any electrode block m block-i +The weight of the cast rod corresponding to this unit m bar-i ).
2. The method for preparing titanium alloy ingots by recycling residual titanium according to claim 1, characterized in that: The length of a single electrode block is 200-600 mm.
3. The method for preparing titanium alloy ingot by recycling residual titanium according to claim 1, characterized in that: In the first vacuum consumable arc melting, the setting value of the DC stirring current is determined by the stirring magnetic field strength it generates, which is 4-6 mT. The AC stirring magnetic field strength during the second vacuum consumable arc melting is 1-3 mT and the stirring period is 4-12 s.
4. The method for preparing titanium alloy ingots by recycling residual titanium according to claim 1, characterized in that: The electrode block has a circular or regular octagonal shape.
5. The method for preparing titanium alloy ingot by recycling residual titanium according to claim 1, characterized in that: The surface cleaning in the above step 1) is specifically performed by using a conventional environmentally friendly degreasing solvent and water to clean the surface in sequence.
6. The method for preparing titanium alloy ingots by recycling residual titanium according to claim 1, characterized in that: The diameter of the center hole of the electrode block is 110-640 mm; and when producing the same ingot, the diameter of the cast rod used is 10-40 mm smaller than the diameter of the center hole of the electrode block; the length of the cast rod is 2000-6000 mm, and the difference between the length of the cast rod and the total length of the electrode block is ≤10 mm.
7. The method for preparing titanium alloy ingot by recycling residual titanium according to claim 1, characterized in that: The outer diameter of the electrode block is 420-880 mm, and the pressing density of the electrode block is 3.2-3.6 g / cm 3 .
8. The method for preparing titanium alloy ingot by recycling residual titanium according to claim 1, characterized in that: In the above composite electrode, the weight of the cast rod accounts for 8-60 wt.% of the weight of the entire composite electrode.
9. The method for preparing titanium alloy ingot by recycling residual titanium according to claim 1, characterized in that: In the above step 2), the power of a single electron gun during melting in the electron beam cold hearth melting furnace is 300-500 kW; the power of a single plasma gun during melting in the plasma beam cold hearth melting furnace is 300-800 kW; the melting current / voltage of the vacuum consumable arc shell furnace is set at 25-55 kA / 25-40V, and the same brand of consumable electrodes with a similar target composition are used during melting; in the above step 4), the melting current / voltage during the first vacuum consumable arc melting is 12-20 kA / 22-28 V; the melting current / voltage during the second vacuum consumable arc melting is 15-30 kA / 24-35 V.
10. The method for preparing titanium alloy ingot by recovering residual titanium according to claim 1 or 2 or 3 or 4 or 5 or 6 or 7 or 8 or 9, characterized in that: The diameter of the titanium alloy ingot finally obtained is 600-1080 mm and the weight is 2000-12000 kg.
Citation Information
Patent Citations
Method for preparing large-specification TC4 titanium alloy cast ingot through high-proportion defective titanium materials
CN108359808A
Titanium alloy cast ingot, preparation method thereof and titanium alloy product
CN115584405A
Method for improving uniformity of al element component in titanium alloy EB ingot
WO2022199508A1