Aluminum alloys and methods of manufacturing the same

By adding rare earth metals such as lanthanum, cerium, strontium, praseodymium to the aluminum alloy, it improves its thermodynamic and physical properties, and the coarse and dissolution of the reinforced phase of aluminum alloy during friction stir welding is solved, and the strength of the welding area is improved. The manufacturing of aluminum alloys through vacuum melting and casting processes achieves effective application and cost reduction in key design spaces.

CN119082568APending Publication Date: 2024-12-06THE BOEING CO
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411246438.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2017-04-11
Filing Date
2018-04-10
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

During friction stir welding, the main reinforced phase of aluminum alloy is coarsized and dissolved at high temperatures, resulting in a decrease in the strength of the welding points, making it difficult to achieve effective manufacturing and manufacturing processes in key design spaces.

Method used

By adding rare earth metals such as lanthanum, cerium, strontium, and praseodymium, the thermodynamic and physical properties of aluminum alloys are improved, the nucleation and reprecipitation of T1 phase are promoted, the strength and material properties of the welding area are improved, and the aluminum alloy is manufactured by vacuum melting and casting technology. .

Benefits of technology

The strength and material properties of the welding area are significantly improved, the strength of the welding points is reduced, the application in more critical design spaces is achieved, and the cost of rare earth elements is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005030903770000031
    Figure BDA0005030903770000031
  • Figure BDA0005030903770000041
    Figure BDA0005030903770000041
  • Figure BDA0005030903770000051
    Figure BDA0005030903770000051
Patent Text Reader

Abstract

The invention relates to an aluminum alloy and a method of making the same. An aluminum alloy includes aluminum, about 1.8 to about 5.6 weight percent copper, about 0.6 to about 2.6 weight percent lithium, and at least one of up to about 1.5 weight percent lanthanum, up to about 1.5 weight percent strontium, up to about 1.5 weight percent cerium, and up to about 1.5 weight percent praseodymium.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application. The application date of the original application is April 10, 2018, the application number is 2018103138134, and the name of the invention is “Aluminum alloy and method for manufacturing the same”. Technical Field

[0002] The present application relates to aluminum alloys, and more particularly to aluminum alloys with additions of copper, lithium, and at least one alkaline earth metal or rare earth metal. Background Art

[0003] Friction stir welding (FSW) is a solid-state joining process that uses a non-consumable tool to join two opposing workpieces without melting the workpiece materials. Friction stir welding generally generates enough heat input during an absolutely solid-state joining process to coarsen and even dissolve the primary strengthening phases in many aluminum alloys. The coarsening and dissolution of the primary precipitates ultimately results in a measurable strength drop across the weld, usually manifested by a typical W-type hardness profile.

[0004] Therefore, those skilled in the art continue their research and development efforts in the field of aluminum alloys. Summary of the invention

[0005] In one embodiment, the disclosed aluminum alloy includes aluminum, about 1.8 to about 5.6 weight percent copper, about 0.6 to about 2.6 weight percent lithium, and at least one of: up to about 1.5 weight percent lanthanum, up to about 1.5 weight percent strontium, up to about 1.5 weight percent cerium, and up to about 1.5 weight percent praseodymium.

[0006] In another embodiment, an aluminum alloy is disclosed that includes aluminum, about 1.8 to about 5.6 weight percent copper, about 0.6 to about 2.6 weight percent lithium, a non-zero amount of at least one of lanthanum, strontium, cerium, and praseodymium up to about 1.5 weight percent each, a non-zero amount of magnesium up to about 1.9 weight percent, a non-zero amount of zirconium up to about 0.16 weight percent, and a non-zero amount of silver up to about 0.7 weight percent.

[0007] In yet another embodiment, an aluminum alloy is disclosed that includes aluminum, from about 1.8 to about 5.6 weight percent copper, from about 0.6 to about 2.6 weight percent lithium, a non-zero amount of at least one of lanthanum, strontium, cerium, and praseodymium up to about 1.5 weight percent each, a non-zero amount of magnesium up to about 1.9 weight percent, a non-zero amount of zirconium up to about 0.16 weight percent, a non-zero amount of silver up to about 0.7 weight percent, a non-zero amount of manganese up to about 0.6 weight percent, a non-zero amount of zinc up to about 1.0 weight percent, and a non-zero amount of titanium up to about 0.15 weight percent.

[0008] In one embodiment, the disclosed method for making an aluminum alloy includes the following steps: (1) weighing a starting material to obtain a material mass, which includes aluminum, about 1.8 to about 5.6 weight percent copper, about 0.6 to about 2.6 weight percent lithium, and at least one of the following: up to about 1.5 weight percent lanthanum, up to about 1.5 weight percent strontium, up to about 1.5 weight percent cerium, and up to about 1.5 weight percent praseodymium; (2) loading the material into a crucible; (3) inserting the crucible into a chamber; (4) evacuating the chamber to a predetermined vacuum level; (5) melting the material to form a melt; and (6) casting the melt into a mold.

[0009] Other embodiments of the disclosed aluminum alloy compositions and methods will become apparent from the following detailed description, the accompanying drawings, and the appended claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1 is a flow chart of aircraft manufacturing and maintenance methods; and

[0011] Figure 2 It is a block diagram of the aircraft. DETAILED DESCRIPTION

[0012] Aluminum alloys are disclosed, which have been improved by adding rare earth metals in the form of lanthanum (La), cerium (Ce), strontium (Sr), praseodymium (Pr), other rare earth or alkaline earth metals, other lanthanides and rare earth metal mixtures (mischmetal), together with various other elements traditionally used for aluminum alloys. For example, aluminum alloys from 2xxx series Al-Cu-Li alloys registered by the Aluminum Association (Aluminum Association) have been improved by adding rare earth ores in the form of La, Ce, Sr, Pr, other rare earth or alkaline earth metals, and rare earth metal mixtures. The disclosed aluminum alloys are designed to produce the dynamic response of materials to friction stir welding (FSW) processes. Without being limited by any specific theory, it is believed that the elements added have three main thermodynamic and physical criteria for improving the properties of the disclosed aluminum alloys, as explained below.

[0013] The T1 phase (the main strengthening phase in the Al-Cu-Li system) is conducive to the distorted lattice sites for nucleation. Therefore, the high strain mismatch produced by these added elements will stimulate the nucleation of the T1 phase. Combined, the criteria described herein produce an ideal scheme for the nucleation and subsequent reprecipitation of the T1 phase during the FSW process. The resulting effect will be a significant improvement in strength and other inherent material properties in the weld zone. Finally, the added elements will eliminate the measurable strength drop commonly observed across the weld zone. This will produce a new category of aluminum alloys that can be implemented in more critical design spaces and are more amenable to desired and effective manufacturing processes (e.g., FSW).

[0014] One general example of the disclosed aluminum alloy has the composition shown in Table 1.

[0015] Table 1

[0016]

[0017] Thus, the aluminum alloys in Table 1 include copper in an amount of about 1.8 to about 5.6 weight percent, lithium in an amount of about 0.6 to about 2.6 weight percent, at least one of lanthanum, strontium, cerium, and praseodymium in a non-zero amount of up to about 1.5 weight percent, wherein each of at least one of lanthanum, strontium, cerium, and praseodymium may be present in a non-zero amount of up to about 1.5 weight percent, and the balance is substantially aluminum. At least one of La, Sr, Ce, and Pr may be derived from a rare earth metal mixture. A rare earth metal mixture is a mixture of rare earth metal ores, typically based on Ce and La, and small amounts of Pr, Sr, and neodymium (Nd), but may contain other lanthanides. Thus, low levels of other lanthanides may also be present in the disclosed aluminum alloys.

[0018] The aluminum alloy of the first embodiment may further include a non-zero amount of up to about 0.20 weight percent or about 0.05 to about 0.20 weight percent of silicon. The aluminum alloy of the first embodiment may further include a non-zero amount of up to about 0.30 weight percent or from about 0.07 to about 0.30 weight percent of iron. The aluminum alloy of the first embodiment may further include a non-zero amount of up to about 0.6 weight percent or about 0.03 to about 0.6 weight percent of manganese. The aluminum alloy of the first embodiment may further include a non-zero amount of up to about 1.9 weight percent or about 0.05 to about 1.9 weight percent of magnesium. The aluminum alloy of the first embodiment may further include a non-zero amount of up to about 0.10 weight percent of chromium. The aluminum alloy of the first embodiment may further include a non-zero amount of up to about 1.0 weight percent or about 0.03 to about 1.0 weight percent of zinc. The aluminum alloy of the first embodiment may further include a non-zero amount of up to about 0.15 weight percent or about 0.07 to about 0.15 weight percent of titanium. The aluminum alloy of the first embodiment may further include a non-zero amount of up to about 0.7 weight percent or from about 0.05 to about 0.7 weight percent of silver. The aluminum alloy of the first embodiment may further include a non-zero amount of up to about 0.16 weight percent or from about 0.04 to about 0.16 weight percent of zirconium. The aluminum alloy of the first embodiment may further include at least one of nickel, gallium, and vanadium in a non-zero amount of each up to about 0.05 weight percent.

[0019] Those skilled in the art will recognize that various impurities may also be present that do not substantially affect the physical properties of the aluminum alloy of the first embodiment, and the presence of such impurities will not result in a departure from the scope of the present disclosure.

[0020] Another general example of the disclosed aluminum alloy has the composition shown in Table 2.

[0021] Table 2

[0022] element Amount (wt.%) Si 0.05-0.20 Cu 1.8-5.6 Fe 0.07–0.30 Mn 0.03–0.6 Mg 0.05–1.9 Cr 0–0.10 Ni 0–0.05 Zn 0–1.0 Ti 0–0.15 Ag 0–0.7 Li 0.6–2.6 Zr 0–0.16 La 0–1.5 Sr 0–1.5 Ce 0–1.5 Pr 0–1.5 Al Approximate margin

[0023] The aluminum alloys in Table 2 include the elements listed and the balance is aluminum or substantially aluminum together with various impurities. In the general example of Table 2, at least one of La, Sr, Ce and Pr must be present in a non-zero amount.

[0024] One specific, non-limiting example of the disclosed aluminum alloy has the composition shown in Table 3.

[0025] Table 3

[0026]

[0027]

[0028] Another specific, non-limiting example of the disclosed aluminum alloy has the composition shown in Table 4.

[0029] Table 4

[0030] element Target (wt.%) Cu 4.07 Fe 0.07 Mn 0.04 Mg 0.37 Zn 0.04 Ti 0.08 Zr 0.13 Ag 0.24 Li 0.94 Sr 0.30 La <0.01 Al margin

[0031] Yet another specific, non-limiting example of the disclosed aluminum alloy has the composition shown in Table 5.

[0032] Table 5

[0033]

[0034]

[0035] The disclosed aluminum alloy can be manufactured by various techniques. A method for manufacturing the disclosed aluminum alloy includes the following steps: (1) weighing the starting material to obtain a material mass within the composition of the aluminum alloy, the aluminum alloy including about 1.8 to about 5.6 weight percent copper, about 0.6 to about 2.6 weight percent lithium, at least one of lanthanum, strontium, cerium and praseodymium each up to about 1.5 weight percent of non-zero amount, and aluminum; (2) loading the material into a crucible; (3) inserting the crucible into a chamber; (4) evacuating the chamber to a predetermined vacuum, wherein the chamber is optionally backfilled with an inert gas; (5) melting the material to form a melt; and (6) casting the melt into a mold. Once the melt is cast into the mold, the melt is cooled to form a solid block, the solid block is homogenized and water quenched to obtain an ingot, the ingot is scalped and hot rolled, and the ingot is solution treated and water quenched, cold rolled or stretched, and artificially or otherwise naturally aged to obtain the aluminum alloy.

[0036] The step of weighing out the starting material may include using a rare earth metal mixture as a source of at least one of lanthanum, strontium, cerium and praseodymium in a non-zero amount of up to about 1.5 weight percent each. A rare earth metal mixture is a mixture of rare earth metal ores, usually based on Ce and La, and a small amount of Pr, Sr and Nd, but possibly containing other lanthanides. A rare earth metal mixture is a cost-effective rare earth element that can be used in the present invention to reduce costs. Rare earth elements are relatively expensive because a large contributor to the cost of rare earth elements is the step of separating the rare earth elements. By utilizing a rare earth metal mixture, the separation step is avoided, so the final product will be less expensive but equally effective.

[0037] In a specific non-limiting example of the disclosed method, the charge material is weighed out and loaded into a graphite crucible. The chamber is then evacuated to a vacuum of less than about 0.05 torr and backfilled with an inert gas (e.g., argon) to a partial pressure of about 760 torr. The charge is melted and cast in a graphite mold and allowed to air cool. The cast ingot can then be homogenized at about 840°F for about 24 hours and water quenched. The ingot can then be peeled and hot rolled to thickness at about 900°F. Then solution treated at 950°F for about 1 hour and water quenched. Finally, cold rolling will be performed, reduced by about 5% and artificially aged. It can be artificially aged at about 310°F for about 32 hours to obtain the aluminum alloy of the present invention.

[0038] Examples of the present disclosure can be found in Figure 1 Aircraft manufacturing and service method 100 shown in Figure 2 1. During pre-production, aircraft manufacturing and service method 100 includes, for example, specification and design 104 of aircraft 102 and material procurement 106. During production, component / subassembly manufacturing 108 and system integration 110 of aircraft 102 takes place. Thereafter, aircraft 102 may be certified and delivered 112 for entry into service 114. While in service by a customer, aircraft 102 is scheduled for routine maintenance and service 116, which may also include modification, reconfiguration, refurbishment, and the like.

[0039] Each process of method 100 may be performed or executed by a system integrator, a third party, and / or an operator (e.g., a customer). For purposes of this description, a system integrator includes, but is not limited to, any number of aircraft manufacturers and major system subcontractors; a third party includes, but is not limited to, any number of suppliers, subcontractors, and vendors; and an operator may be an airline, a leasing company, a military entity, a service organization, and the like.

[0040] like Figure 2 , the aircraft 102 produced by the example method 100 includes, for example, an airframe 118 and an interior 122 having a plurality of systems 120. Examples of the plurality of systems 120 include one or more of a propulsion system 124, an electrical system 126, a hydraulic system 128, and an environmental system 130. Any number of other systems may be included.

[0041] The disclosed aluminum alloy compositions and articles formed therefrom can be employed during any one or more stages of the aircraft manufacturing and maintenance method 100. As an example, components or subcomponents corresponding to component / subcomponent manufacturing 108, system integration 110, and / or maintenance and service 116 can be processed or manufactured using the disclosed aluminum alloy compositions. As another example, the fuselage 118 can be constructed using the disclosed aluminum alloy compositions. Moreover, one or more device instances, method instances, or combinations thereof can be used during component / subcomponent manufacturing 108 and / or system integration 110, for example, by significantly speeding up or reducing the cost of assembly of the aircraft 102, such as the fuselage 118 and / or the interior 122. Similarly, one or more of the system instances, method instances, or combinations thereof can be used when the aircraft 102 is in service, such as and not limited to maintenance and service 116.

[0042] Further aspects are described according to the following clauses:

[0043] Clause 1. An aluminum alloy comprising:

[0044] aluminum;

[0045] about 1.8 to about 5.6 weight percent copper;

[0046] From about 0.6 to about 2.6 weight percent lithium; and

[0047] At least one of the following:

[0048] Up to about 1.5 weight percent lanthanum;

[0049] Up to about 1.5 weight percent strontium;

[0050] Up to about 1.5 weight percent cerium; and

[0051] Up to about 1.5 weight percent praseodymium.

[0052] Item 2. The aluminum alloy of Item 1, comprising at least two of the lanthanum, the strontium, the cerium, and the praseodymium.

[0053] Clause 3. The aluminum alloy of clause 1 or 2, further comprising at least one of the following:

[0054] a non-zero amount of up to about 0.20 weight percent silicon;

[0055] a non-zero amount of up to about 0.30 weight percent iron;

[0056] a non-zero amount of up to about 0.6 weight percent manganese;

[0057] a non-zero amount of up to about 1.9 weight percent magnesium;

[0058] a non-zero amount of up to about 0.10 weight percent chromium;

[0059] a non-zero amount of up to about 1.0 weight percent zinc;

[0060] a non-zero amount of up to about 0.15 weight percent titanium;

[0061] a non-zero amount of up to about 0.7 weight percent silver; and

[0062] A non-zero amount of zirconium up to about 0.16 weight percent.

[0063] Clause 4. The aluminum alloy of any of Clauses 1-3, further comprising at least one of: up to about 0.05 weight percent nickel, up to about 0.05 weight percent gallium, and up to about 0.05 weight percent vanadium.

[0064] Clause 5. The aluminum alloy of any one of clauses 1-4, further comprising:

[0065] a non-zero amount of up to about 1.9 weight percent magnesium;

[0066] a non-zero amount of up to about 0.16 weight percent zirconium; and

[0067] A non-zero amount of silver up to about 0.7 weight percent.

[0068] Clause 6. The aluminum alloy of any one of Clauses 1-5, comprising said strontium.

[0069] Clause 7. The aluminum alloy of any of Clauses 1-6, comprising said lanthanum.

[0070] Clause 8. The aluminum alloy of any one of Clauses 1-7, comprising said cerium.

[0071] Clause 9. The aluminum alloy of any one of Clauses 1-8, comprising said praseodymium.

[0072] Clause 10. The aluminum alloy of any one of clauses 1-9, further comprising:

[0073] a non-zero amount of up to about 1.9 weight percent magnesium;

[0074] a non-zero amount of up to about 0.16 weight percent zirconium;

[0075] a non-zero amount of up to about 0.7 weight percent silver;

[0076] a non-zero amount of up to about 0.6 weight percent manganese;

[0077] a non-zero amount of up to about 1.0 weight percent zinc; and

[0078] A non-zero amount of titanium up to about 0.15 weight percent.

[0079] Clause 11. A method for producing an aluminum alloy, comprising the steps of:

[0080] Weighing the starting material to obtain a mass of material having the composition of clause 1;

[0081] loading the starting materials into a crucible;

[0082] inserting the crucible into a chamber;

[0083] evacuating the chamber to a predetermined vacuum level;

[0084] melting the starting materials to form a melt; and

[0085] The melt is cast into a mold.

[0086] Clause 12. The method of Clause 11, wherein the predetermined vacuum level is at most about 0.05 Torr, and wherein the chamber is backfilled with an inert gas.

[0087] Clause 13. The method of clause 11 or 12, wherein:

[0088] casting the melt into a mold;

[0089] allowing the melt to cool to form a solid mass;

[0090] homogenizing and water quenching the solid mass to obtain an ingot;

[0091] peeling and hot rolling the ingot;

[0092] The ingot is at least one of solution treated, cold rolled and stretched; and

[0093] The ingot was aged.

[0094] Clause 14. The method of any of Clauses 11-13, wherein the ingot is artificially aged at about 300 to about 320° F. for about 29 to about 35 hours.

[0095] Clause 15. The method of any of Clauses 11-14, wherein the weighing comprises weighing a mischmetal as a source of the at least one of the lanthanum, the strontium, the cerium, and the praseodymium.

[0096] The disclosed aluminum alloy compositions and articles formed therefrom are described in the context of aircraft; however, one of ordinary skill in the art will readily recognize that the disclosed aluminum alloy compositions and articles formed therefrom can be used in a variety of applications. For example, the disclosed aluminum alloy compositions and articles formed therefrom can be implemented in various types of vehicles, including, for example, helicopters, passenger ships, automobiles, marine products (boats, motors, etc.), and the like.

[0097] While various embodiments of the disclosed aluminum alloy compositions and articles formed therefrom have been shown and described, modifications will occur to those skilled in the art upon reading the specification. The present application includes such modifications and is limited only by the scope of the claims.

Claims

1. A method for producing an aluminum alloy, comprising: subjecting an aluminum alloy to a solid state joining process, wherein the aluminum alloy comprises: aluminum; about 1.8 to about 5.6 weight percent copper; From about 0.6 to about 2.6 weight percent lithium; and at least one of lanthanum, cerium and praseodymium in an amount ranging from 0.5 weight percent to about 1.5 weight percent, wherein a T1 phase is precipitated during the solid state joining process; and Prior to the solid state joining process, the aluminum is aged.

2. The method of claim 1, wherein the solid-state joining process comprises friction stir welding.

3. The method of claim 1 wherein aging the aluminum prior to the solid state joining process comprises artificial aging at about 300 to about 320°F for about 29 to about 35 hours.

4. The method of claim 1, wherein the aluminum alloy further comprises a non-zero amount of titanium up to about 0.15 weight percent.

5. The method of claim 1, wherein the aluminum alloy further comprises a non-zero amount of silver up to about 0.7 weight percent.

6. The method of claim 1, wherein the aluminum alloy further comprises a non-zero amount of silicon up to about 0.20 weight percent.

7. The method of claim 1, wherein the aluminum alloy further comprises a non-zero amount of iron up to about 0.30 weight percent.

8. The method of claim 1, wherein the aluminum alloy further comprises a non-zero amount of manganese up to about 0.6 weight percent.

9. The method of claim 1, wherein the aluminum alloy further comprises a non-zero amount of chromium up to about 0.10 weight percent.

10. The method of claim 1, wherein the aluminum alloy further comprises a non-zero amount of zirconium up to about 0.16 weight percent.

11. The method of claim 1, wherein the aluminum alloy further comprises at least one of: up to about 0.05 weight percent nickel, up to about 0.05 weight percent gallium, and up to about 0.05 weight percent vanadium.

12. The method of claim 1, wherein the aluminum alloy further comprises a non-zero amount of magnesium up to about 1.9 weight percent.

13. The method of claim 1, wherein the aluminum alloy further comprises magnesium in a range of about 0.05 to about 1.9 weight percent.

14. The method of claim 1, wherein the aluminum alloy further comprises a non-zero amount of zinc up to about 1.0 weight percent.

15. The method of claim 1, wherein the aluminum alloy further comprises zinc in a range of about 0.03 to about 1.0 weight percent.

16. The method of claim 1, wherein at least one of lanthanum and praseodymium is in a range of 0.5 weight percent to about 1.5 weight percent.

17. The method of claim 16, wherein the aluminum alloy further comprises a non-zero amount of magnesium up to about 1.9 weight percent.

18. The method of claim 16, wherein the aluminum alloy further comprises magnesium in a range of about 0.05 to about 1.9 weight percent.

19. The method of claim 16, wherein the aluminum alloy further comprises a non-zero amount of zinc up to about 1.0 weight percent.

20. The method of claim 16, wherein the aluminum alloy further comprises zinc in a range of about 0.03 to about 1.0 weight percent.

Citation Information

Patent Citations

  • Scandium and strontium compound microalloyed high zinc 2099 type aluminium alloy and preparation method thereof

    CN101838764A

  • Aluminum-zinc-magnesium-silver alloy

    CN101910443A

  • High strength aluminum alloy

    US20020134474A1

  • Aluminum-lithium alloys

    US4832910A

  • Ultra high strength aluminum-base alloys

    US5211910A