Mg-Al-Mn-Ca-Sb quinary heat-resistant magnesium alloy and preparation method thereof

By adding Ca and Sb to the Mg-Al-Mn alloy, the process is optimized to form a high melting point phase, the problem of insufficient thermal stability of magnesium alloy is solved, and the low-cost and high-performance Mg-Al-Mn-Ca- is achieved. Sb five-member alloy, suitable for high-temperature environments such as rail transit.

CN119082571APending Publication Date: 2024-12-06CRRC CHANGCHUN RAILWAY VEHICLES CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411203341.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing magnesium alloys have insufficient thermal stability in the field of rail transit, which has limited its application in high temperature environments, and the high cost of adding rare earth elements, which limits its wide application.

Method used

Using Mg-Al-Mn-Ca-Sb five-membered alloy, the content is adjusted by adding Ca and Sb to the Mg-Al-Mn alloy, and optimized through solid solution treatment and symmetric extrusion process to form high melting points CaMgSb and Ca2Sb. phase, improve the mechanical properties and thermal stability of the alloy.

Benefits of technology

It has achieved excellent mechanical properties of magnesium alloys at room temperature and high temperatures, especially the improvement of high-temperature creep resistance, and is low in cost and does not contain rare earth elements, making them suitable for commercial applications.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides an Mg-Al-Mn-Ca-Sb five-element heat-resistant magnesium alloy which comprises the following components in percentage by mass: 3 to 4 percent of Al, 0.4 to 0.5 percent of Mn, 0.6 to 0.7 percent of Ca, 0.1 to 0.3 percent of Sb and the balance of Mg. The invention further provides a preparation method of the Mg-Al-Mn-Ca-Sb five-component heat-resistant magnesium alloy. According to the Mg-Al-Mn-Ca-Sb quinary heat-resistant magnesium alloy provided by the invention, the Ca element and the Sb element are added on the basis of an Mg-Al-Mn system, and the content of the alloy elements is adjusted, so that the magnesium alloy has higher room-temperature mechanical properties and thermal stability; furthermore, proper smelting, pouring, solid solution, aging and symmetric extrusion processes are matched for alloying design, and the heat-resistant magnesium alloy is obtained through the interaction among elements and the synergistic effect of extrusion deformation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of technical materials, and in particular to a Mg-Al-Mn-Ca-Sb five-element heat-resistant magnesium alloy and a preparation method thereof. Background Art

[0002] As one of the lightest high-performance materials discovered so far, magnesium alloy has the advantages of high specific strength and specific stiffness. In addition, its castability, electrical and thermal conductivity, and cutting performance are also relatively good. Therefore, magnesium alloy is widely used in the automotive, electronic and electrical, aerospace and other fields.

[0003] At present, in the field of rail transit, magnesium alloy, as the metal material with the lowest density, is an effective way to achieve lightweight body structure. However, magnesium alloy is a very active metal material, especially in practical applications, magnesium alloy must have a certain thermal stability; however, most commercial magnesium alloys have poor thermal stability. Most of the magnesium alloys reported with certain thermal stability have added various rare earth elements, such as ZE41 and WE43 alloys with excellent room temperature and high temperature tensile and creep properties. ZE41 provides medium strength at a temperature of up to 150 ° C, and WE43 alloy can provide good mechanical properties at a temperature of up to 250 ° C. However, the addition of rare earth elements is too expensive for the widespread application of magnesium alloys. Therefore, this type of magnesium alloy is currently mainly used in aerospace. Therefore, it is very necessary to explore a low-cost, high thermal stability magnesium alloy for commercial applications.

[0004] Mg-Al-Mn alloys are low in cost and have excellent performance in all aspects. As the Al content in the alloy increases, the strength and ductility of the Mg-Al alloy increase simultaneously. In order to improve the performance of Mg alloys and expand their application needs, it is of great significance to provide a magnesium alloy with heat resistance, high strength and high plasticity based on the Mg-Al-Mn alloys. Summary of the invention

[0005] The technical problem solved by the present invention is to provide a Mg-Al-Mn-Ca-Sb five-element heat-resistant magnesium alloy. The magnesium alloy provided by the present application has excellent mechanical properties at room temperature and high temperature.

[0006] In view of this, the present application provides a Mg-Al-Mn-Ca-Sb quinary heat-resistant magnesium alloy, which includes, by mass percentage, 3-4% Al, 0.4-0.5% Mn, 0.6-0.7% Ca, 0.1-0.3% Sb, and the balance Mg.

[0007] Preferably, the content of Al is 4%, and the content of Mn is 0.5%.

[0008] Preferably, the content of Ca is 0.6%, and the content of Sb is 0.1%.

[0009] Preferably, the content of Ca is 0.7%, and the content of Sb is 0.2%.

[0010] Preferably, the content of Ca is 0.7%, and the content of Sb is 0.3%.

[0011] The present application also provides a method for preparing the five-element heat-resistant magnesium alloy, comprising the following steps:

[0012] S1) preheating pure Mg, pure Al, Mg-15Mn master alloy, Mg-20Ca master alloy and Mg-20Sb master alloy respectively, mixing the preheated raw materials according to the component ratio and then smelting them, and casting them to obtain magnesium alloy ingots;

[0013] S2) subjecting the magnesium alloy ingot to a solution treatment, an aging treatment, and then a symmetrical extrusion treatment to obtain a five-element heat-resistant magnesium alloy.

[0014] Preferably, the preheating temperature is 270-310° C. and the preheating time is 10-15 minutes.

[0015] Preferably, the smelting is carried out in a mixed gas of CO2 and SF6, the smelting temperature is 660-710°C, and the smelting time is 10-20 minutes.

[0016] Preferably, the temperature of the solution treatment is 400-450° C., and the time is 15-20 h; the temperature of the aging treatment is 200-300° C., and the time is 10-15 h.

[0017] Preferably, the temperature of the symmetrical extrusion treatment is 220-250° C., the speed is 0.4-1.2 mm / s, and the extrusion ratio is 20-30.

[0018] The present application provides a Mg-Al-Mn-Ca-Sb five-element heat-resistant magnesium alloy, which comprises, by mass percentage, 3-4% Al, 0.4-0.5% Mn, 0.6-0.7% Ca, and 0.6-0.7% Sb. 0.1~0.3%, the balance is Mg; in the five-element heat-resistant magnesium alloy provided by the present application, Ca can inhibit grain growth, increase the density of the precipitated phase, and weaken the texture, thereby improving the mechanical properties of the magnesium alloy. At the same time, the addition of Ca can form a dense CaO-MgO layer on the surface of the magnesium alloy to prevent Mg vapor from diffusing outward and causing fire; Sb can improve the cast structure of the magnesium alloy and make the coarse dendrites finer, and Sb will also form a dispersed second phase Mg3Sb2 with Mg. The Mg3Sb2 phase has a high melting point, good thermal stability and strengthens the grain boundaries, so that the room temperature and high temperature mechanical properties of the magnesium alloy are improved to a certain extent, especially the high temperature creep resistance is greatly improved, and the plasticity is not significantly damaged; further, the solubility of Ca and Sb elements in Mg is relatively low, and the formed (Mg, Al)2Ca and Ca2Sb phases are distributed at the grain boundaries as heat-resistant phases. Therefore, the Mg-Al-Mn-Ca-Sb five-element magnesium alloy provided by the present application has higher room temperature tensile properties and thermal stability. DETAILED DESCRIPTION

[0019] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.

[0020] In view of the performance requirements of heat resistance, high strength and high plasticity of Mg-Al-Mn magnesium alloys in the prior art, the present application provides a Mg-Al-Mn-Ca-Sb five-element magnesium alloy, which adds Ca and Sb to the Mg-Al-Mn magnesium alloy and adjusts the addition amount so that the obtained magnesium alloy has excellent tensile strength, yield strength and elongation at room temperature and high temperature, thereby ensuring the excellent heat resistance of the magnesium alloy. Specifically, the embodiment of the present invention discloses a Mg-Al-Mn-Ca-Sb five-element heat-resistant magnesium alloy, which includes, by mass percentage: Al 3-4%, Mn 0.4-0.5%, Ca 0.6-0.7%, Sb 0.1-0.3%, and the balance Mg.

[0021] In the magnesium alloy provided in the present application, the Al content is 3-4%. In a specific embodiment, the Al content is 4%. At this content, the Al content is in a medium alloy system, and the extrusion performance of the magnesium alloy is good.

[0022] The content of Mn is 0.4-0.5%. In a specific embodiment, the content of Mn is 0.5%. The above content of Mn under the same content ratio makes the magnesium alloy have excellent heat resistance.

[0023] The content of Ca is 0.6-0.7%, specifically, the content of Ca is 0.6% or 0.7%; Ca can generate CaMgSb phase in Mg-Al-Sb system, and through a reasonable solid solution process, Ca element is dissolved into the matrix as much as possible to spheroidize the high melting point CaMgSb phase; and the solubility of Ca element and Sb element in Mg is low, and the (Mg, Al)2Ca and Ca2Sb phases generated at the same time are heat-resistant phases; further, combined with the symmetrical extrusion process, the grains of the heat-resistant CaMgSb phase and the heat-resistant Ca2Sb phase are refined, and the texture is weakened, so that the mechanical properties and heat resistance of the alloy are greatly enhanced.

[0024] The content of Sb is 0.1-0.3%, specifically, the content of Sb is 0.1%, 0.2%, and 0.3%; the addition of Sb can improve the cast structure of the magnesium alloy and make the coarse dendrites finer, and Sb will also form a dispersed second phase Mg3Sb2 with Mg, which has a high melting point, good thermal stability and strengthens the grain boundaries, so that the room temperature and high temperature mechanical properties of the magnesium alloy are improved to a certain extent, especially the high temperature creep resistance is greatly improved, and the plasticity is not significantly damaged; further, the solubility of Ca and Sb elements in Mg is low, and the (Mg, Al)2Ca and Ca2Sb phases generated at the same time are heat-resistant phases, and the large deformation process of symmetrical extrusion can make the grains refined again, and play a role in weakening the texture. This design makes the alloy composition contain no rare earth elements, and while saving costs, a heat-resistant magnesium alloy with excellent performance is obtained through alloy optimization and symmetrical extrusion.

[0025] In the magnesium alloy provided in the present application, for example, the Al content is 4%, the Mn content is 0.5%, the Ca content is 0.6%, the Sb content is 0.1%, and the balance is Mg, or, the Al content is 4%, the Mn content is 0.5%, the Ca content is 0.7%, the Sb content is 0.2%, and the balance is Mg, or, the Al content is 4%, the Mn content is 0.5%, the Ca content is 0.7%, the Sb content is 0.3%, and the balance is Mg.

[0026] Furthermore, the present application also provides a method for preparing a five-element heat-resistant magnesium alloy, comprising the following steps:

[0027] S1) preheating pure Mg, pure Al, Mg-15Mn master alloy, Mg-20Ca master alloy and Mg-20Sb master alloy respectively, mixing the preheated raw materials according to a mass ratio and then smelting them, and casting them to obtain a magnesium alloy ingot;

[0028] S2) subjecting the magnesium alloy ingot to a solution treatment, an aging treatment, and then a symmetrical extrusion treatment to obtain a five-element heat-resistant magnesium alloy.

[0029] In the preparation process of the five-element heat-resistant magnesium alloy, the raw materials pure Mg, pure Al, Mg-15Mn master alloy, Mg-20Ca and Mg-20Sb master alloy are first preheated respectively, and the preheating temperature is 270-310°C and the time is 10-15min. Specifically, the preheating temperature is 280-300°C and the time is 11-14min. More specifically, the preheating temperature is 290°C and the time is 12min.

[0030] The present application then mixes the preheated raw materials according to the mass ratio, and then melts and pours them to obtain a magnesium alloy ingot; the melting and pouring process is specifically as follows:

[0031] The preheated raw materials are mixed under the protection of a mixed gas of CO2 and SF6, and the temperature is heated to 660-710°C and kept warm for 10-20 minutes. After the alloy is melted, argon gas is introduced and stirred for 2 minutes to promote uniform mixing of the melt and achieve the effect of degassing the melt. The raw materials are allowed to stand at this temperature for 5 minutes to allow impurities to float, and finally the slag is skimmed off and the magnesium alloy ingot is cast.

[0032] Specifically, the heating temperature is 680-700° C., and the insulation time is 14-16 minutes; more specifically, the heating temperature is 700° C., and the insulation time is 15 minutes; the volume ratio of the above-mentioned mixed gas CO2 and SF6 is 90:1.

[0033] According to the present invention, the magnesium alloy ingot is then subjected to solution treatment and aging treatment in sequence, wherein the temperature of the solution treatment is 400-450°C, and the time is 15-20 hours. Specifically, the temperature of the solution treatment is 400-430°C, and the time is 14-16 hours. The temperature of the aging treatment is 200-300°C, and the time is 10-15 hours. Specifically, the temperature of the aging treatment is 220-250°C, and the time is 10-13 hours. More specifically, the temperature of the solution treatment is 420°C, and the time is 16 hours. The temperature of the aging treatment is 230°C, and the time is 12 hours.

[0034] Finally, the present application performs symmetrical extrusion treatment on the magnesium alloy after aging treatment, wherein the temperature of the symmetrical extrusion treatment is 220-250°C, the rate is 0.4-1.2 mm / s, and the extrusion ratio is 20-30; specifically, the temperature of the symmetrical extrusion treatment is 240°C, the rate is 1.0 mm / s, and the extrusion ratio is 25.

[0035] In order to further understand the present invention, the Mg-Al-Mn-Ca-Sb quinary heat-resistant magnesium alloy and the preparation method thereof provided by the present invention are described in detail below in conjunction with the embodiments. The protection scope of the present invention is not limited by the following embodiments.

[0036] Example 1

[0037] In this embodiment, the heat-resistant magnesium alloy contains the following components in mass percentage: Al: 4%, Mn: 0.5%, Ca: 0.6wt%, Sb: 0.1%, and the rest are Mg and unavoidable impurity elements.

[0038] In this embodiment, the method for preparing the heat-resistant magnesium alloy comprises the following steps:

[0039] 1) preheating pure Mg, pure Al, Mg-15Mn master alloy, Mg-20Ca master alloy and Mg-20Sb master alloy at a preheating temperature of 290° C. for 12 minutes;

[0040] 2) Preheating pure Mg, pure Al, Mg-15Mn master alloy, Mg-20Ca master alloy and Mg-20Sb master alloy according to mass ratio is mixed and smelted under the protection of a mixed gas of CO2 and SF6 with a volume ratio of about 90:1, the temperature is heated to 700°C, and the temperature is kept for 15 minutes. After the alloy is melted, argon gas is introduced and stirred for 2 minutes to promote uniform mixing of the melt and achieve the effect of degassing the melt. At this temperature, it is allowed to stand for 5 minutes to allow impurities to float, and finally the slag is skimmed off and cast to obtain a magnesium alloy ingot;

[0041] 3) The cast magnesium alloy ingot is subjected to solution treatment and aging treatment in sequence, firstly the temperature is raised to 410°C, kept at this temperature for 16 hours, and then aged at 200°C for 10 hours;

[0042] 4) The magnesium alloy ingot after aging treatment is extruded under the extrusion conditions of an extrusion temperature of 240° C., an extrusion rate of 1.0 mm / s, and an extrusion ratio of 25 to obtain a five-element heat-resistant magnesium alloy.

[0043] The yield strength of the magnesium alloy at room temperature is 310 MPa, the tensile strength is 345 MPa, and the elongation is 15.8%; at a temperature of 180° C., the yield strength is 270 MPa, the tensile strength is 318 MPa, and the elongation is 31%.

[0044] Example 2

[0045] In this embodiment, the heat-resistant magnesium alloy contains the following components in mass percentage: Al: 4%, Mn: 0.5%, Ca: 0.7wt%, Sb: 0.2%, and the rest are Mg and unavoidable impurity elements.

[0046] In this embodiment, the method for preparing the heat-resistant magnesium alloy comprises the following steps:

[0047] 1) preheating pure Mg, pure Al, Mg-15Mn master alloy, Mg-20Ca master alloy and Mg-20Sb master alloy at a preheating temperature of 290° C. for 12 minutes;

[0048] 2) Preheating pure Mg, pure Al, Mg-15Mn master alloy, Mg-20Ca master alloy and Mg-20Sb master alloy is mixed and smelted according to the mass ratio under the protection of a mixed gas of CO2 and SF6 with a volume ratio of about 90:1, and the temperature is heated to 700°C and kept warm for 15 minutes. After the alloy is melted, argon gas is introduced and stirred for 2 minutes to promote uniform mixing of the melt and achieve the effect of degassing the melt. The alloy is allowed to stand at this temperature for 5 minutes to allow impurities to float, and finally the slag is skimmed off and cast to obtain a magnesium alloy ingot;

[0049] 3) The cast magnesium alloy ingot is subjected to solution treatment and aging treatment in sequence, firstly the temperature is raised to 410°C and kept for 16 hours, and then aged at 200°C for 10 hours;

[0050] 4) The magnesium alloy ingot after aging treatment was symmetrically extruded under the extrusion conditions of extrusion temperature of 240° C., extrusion rate of 1.0 mm / s, and extrusion ratio of 25 to obtain a five-element magnesium alloy.

[0051] The yield strength of the magnesium alloy at room temperature is 318 MPa, the tensile strength is 360 MPa, and the elongation is 16.1%; at a temperature of 180° C., the yield strength is 283 MPa, the tensile strength is 326 MPa, and the elongation is 31.5%.

[0052] Example 3

[0053] In this embodiment, the heat-resistant magnesium alloy contains the following components in mass percentage: Al: 4%, Mn: 0.5%, Ca: 0.7wt%, Sb: 0.3%, and the rest are Mg and unavoidable impurity elements.

[0054] In this embodiment, the method for preparing the heat-resistant magnesium alloy comprises the following steps:

[0055] 1) preheating pure Mg, pure Al, Mg-15Mn master alloy, Mg-20Ca master alloy and Mg-20Sb master alloy respectively at a preheating temperature of 290° C. for 12 minutes;

[0056] 2) Pure Mg, pure Al, Mg-15Mn master alloy, Mg-20Ca master alloy and Mg-20Sb master alloy are mixed and smelted in accordance with the mass ratio under the protection of a mixed gas of CO2 and SF6 with a volume ratio of about 90:1, the temperature is heated to 700°C, and the temperature is kept for 15 minutes. After the alloy is melted, argon gas is introduced and stirred for 2 minutes to promote uniform mixing of the melt and achieve the effect of degassing the melt. The alloy is allowed to stand at this temperature for 5 minutes to allow impurities to float, and finally the slag is skimmed off and the magnesium alloy ingot is cast;

[0057] 3) The cast magnesium alloy ingot is subjected to solution treatment and aging treatment in sequence; the temperature is first raised to 410°C, kept at this temperature for 16 hours, and then kept at 200°C for 10 hours;

[0058] 4) The magnesium alloy ingot after aging treatment was symmetrically extruded under the extrusion conditions of extrusion temperature of 240° C., extrusion rate of 1.0 mm / s, and extrusion ratio of 25 to obtain a five-element magnesium alloy.

[0059] The yield strength of the magnesium alloy at room temperature is 325 MPa, the tensile strength is 368 MPa, and the elongation is 17%; at a temperature of 180° C., the yield strength is 293 MPa, the tensile strength is 336 MPa, and the elongation is 32%.

[0060] By comparing Example 1, Example 2, and Example 3, it can be found that with the increase of the content of the two elements Ca and Sb, the decrease degree of the tensile strength and the yield strength at high temperature decreases, and the room temperature mechanical properties and the high temperature tensile properties gradually improve, indicating that the addition of the two elements Ca and Sb can make the magnesium alloy have good thermal stability.

[0061] Example 1, Example 2, Example 3 are compared with the prior art:

[0062] In the prior art, a Chinese patent with publication number CN116103549A provides an ultrafine-grained magnesium alloy containing Mn and Sb and a preparation method thereof, which discloses that the content of the magnesium alloy is Mn: 0.93%, Sb: 1.12%, and the rest is Mg; the yield strength of the magnesium alloy in the extruded state is 196MPa, the tensile strength is 245MPa, and the elongation is 23.3%;

[0063] The Chinese patent with publication number CN116065070A provides a high-strength and toughness magnesium alloy and a preparation method thereof, which discloses that the room temperature tensile properties of the extruded Mg-1Sb-1Mn-1Sn-0.2Zn alloy are as follows: yield strength is 301MPa, tensile strength is 361Mpa, and elongation is 23.3%;

[0064] The Chinese patent with publication number CN104480361A provides a high-strength and tough heat-resistant die-casting magnesium alloy and a preparation method thereof, which discloses a magnesium alloy system of 6.5% Al, 0.97% Ca, 0.8% Sn, 0.4% Mn, Zn≤0.02%, impurity element Si≤0.03%, other impurities (Fe+Ni+Cu)≤0.01%, and the balance is Mg. The magnesium alloy has a tensile strength of 276.8 MPa, a yield strength of 173.4 MPa, and an elongation of 9.9% at room temperature, and a tensile strength of 186.5 MPa, a yield strength of 135.8 MPa, and an elongation of 16.3% at a temperature of 150°C;

[0065] Zhang Mingquan et al. published a paper entitled "The Effect of Ca and Al Mass Ratio on the Microstructure and Properties of Mg-Al-Ca-Mn Alloy" in the journal "Special Casting and Nonferrous Alloys". They disclosed that the yield strength of the cast Mg-3Al-4Ca-0.4Mn alloy is 123MPa, the tensile strength is 149MPa, and the elongation is 1.1%;

[0066] In a paper titled "Effect of Sb Low Alloying on Microstructure and Mechanical Properties of Mg-9Al-based Alloy" published in the journal "Journal of the Chinese Society of Nonferrous Metals", Yuan Guangyin et al. proposed that the mechanical properties of Mg-9Al-0.8Zn-0.2Mn-0.35Sb magnesium alloy at room temperature are: yield strength of 172MPa, tensile strength of 264MPa, and elongation of 4.5%; the yield strength at a temperature of 150°C is 138MPa, the tensile strength is 165MPa, and the elongation is 34%.

[0067] Through the data comparison and analysis of the above data, in the embodiments 1, 2 and 3 of the present invention, Ca and Sb elements are added in the Mg-Al-Mn alloy system to significantly improve the mechanical properties of the alloy and the thermal stability at high temperature. The extruded magnesium alloy prepared by the present invention forms a Mg3Sb2 strengthening matrix after the intervention of Sb as an alloying element of the magnesium alloy through the mutual synergistic effect of Ca and Sb in the Mg-Al-Mn alloy system. Mg3Sb2 is a heat-resistant intermetallic compound, which has the characteristics of high strength, high hardness, good ductility and good corrosion resistance. Ca can also improve the mechanical properties of the magnesium alloy by inhibiting grain growth, increasing the density of the precipitated phase, weakening the texture and a series of mechanisms, and Ca can improve the thermal stability in the casting process and improve the yield rate of the cast magnesium alloy, which makes the alloy have excellent mechanical properties at high temperature (yield strength of 270-293MPa, tensile strength of 318-336MPa, elongation of 31%-32%).

[0068] The above embodiments are only used to help understand the method and core idea of ​​the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

[0069] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A Mg-Al-Mn-Ca-Sb five-element heat-resistant magnesium alloy, comprising, by mass percentage: Al 3~4%, Mn 0.4~0.5%, Ca 0.6~0.7%, Sb 0.1~0.3%, and the balance Mg.

2. The five-element heat-resistant magnesium alloy according to claim 1, characterized in that: The content of Al is 4%, and the content of Mn is 0.5%.

3. The five-element heat-resistant magnesium alloy according to claim 2, characterized in that: The content of Ca is 0.6%, and the content of Sb is 0.1%.

4. The five-element heat-resistant magnesium alloy according to claim 2, characterized in that: The content of Ca is 0.7%, and the content of Sb is 0.2%.

5. The five-element heat-resistant magnesium alloy according to claim 2, characterized in that: The content of Ca is 0.7%, and the content of Sb is 0.3%.

6. The method for preparing the five-element heat-resistant magnesium alloy according to claim 1, comprising the following steps: S1) preheating pure Mg, pure Al, Mg-15Mn master alloy, Mg-20Ca master alloy and Mg-20Sb master alloy respectively, mixing the preheated raw materials according to the component ratio and then smelting them, and casting them to obtain magnesium alloy ingots; S2) subjecting the magnesium alloy ingot to a solution treatment, an aging treatment, and then a symmetrical extrusion treatment to obtain a five-element heat-resistant magnesium alloy.

7. The preparation method according to claim 6, characterized in that: The preheating temperature is 270-310° C. and the preheating time is 10-15 minutes.

8. The preparation method according to claim 6, characterized in that: The smelting is carried out in a mixed gas of CO2 and SF6, the smelting temperature is 660-710°C, and the smelting time is 10-20 minutes.

9. The preparation method according to claim 6, characterized in that: The temperature of the solution treatment is 400-450° C., and the time is 15-20 hours; the temperature of the aging treatment is 200-300° C., and the time is 10-15 hours.

10. The preparation method according to claim 6, characterized in that: The temperature of the symmetrical extrusion process is 220-250° C., the speed is 0.4-1.2 mm / s, and the extrusion ratio is 20-30.