High-strength and high-oxidation-resistance refractory high-entropy alloy and preparation method thereof

By designing PtxCrTaTi high-entropy alloy and vacuum arc smelting process, the existing high-temperature alloys have poor oxidation resistance and high cost of precious metals have been solved, and a refractory high-entropy alloy with high strength and excellent high-temperature oxidation resistance is achieved, which is suitable for high-temperature applications.

CN119082583APending Publication Date: 2024-12-06YUNNAN PRECIOUS METALS LAB CO LTD +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411232894.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing refractory high-temperature alloys are difficult to form dense oxide films at high temperatures, resulting in poor high-temperature oxidation resistance. The development of precious metal alloys is limited by high prices and severe oxidation volatility.

Method used

PtxCrTaTi high-entropy alloy was designed. Through reasonable alloy composition ratio and vacuum arc smelting process, an oxide layer was formed to prevent oxidation volatility and oxygen and nitrogen penetration. Combined with water-cooled copper mold crucible smelting technology, the uniformity of alloy smelting and reduce the amount of precious metals used. .

Benefits of technology

It significantly improves the high-temperature oxidation resistance and strength. The alloy exhibits excellent oxidation stability and uniformity under 1200°C, reducing manufacturing costs and is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082583A_ABST
    Figure CN119082583A_ABST
Patent Text Reader

Abstract

The invention discloses a high-strength and high-oxidation-resistance refractory high-entropy alloy and a preparation method thereof, and belongs to the technical field of high-entropy alloys. The molar ratio of Pt to Cr to Ta to Ti is x: 1: 1: 1, x is 0.1-1, and the preparation method comprises the following steps: (1) pretreatment; and (2) vacuum arc melting. According to the invention, through reasonable alloy component design and combination of a proper preparation method, the alloy with better strength, high-temperature oxidation performance and uniformity is prepared on the basis of lower cost, so that the alloy can meet higher use requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high entropy alloys, and relates to a high-strength and high-oxidation-resistant refractory high entropy alloy and a preparation method thereof. Background Art

[0002] With the rapid development of aero engines and gas turbines, higher requirements are placed on the performance of high-temperature materials. However, the widely used nickel-based high-temperature alloys have an inherent melting point (1300°C) limitation, making it difficult to meet higher usage requirements. Precious metal alloys (such as PtIr alloys and PtRh alloys) have higher melting points and excellent oxidation resistance, but iridium, rhodium, and platinum are all precious metals, which are expensive and have serious oxidation volatilization during use, thus limiting their development. In recent years, the concept of high-entropy alloys has been proposed, which are usually composed of four or more elements in equal or non-equal molar ratios. Among them, refractory high-entropy alloys have attracted widespread attention due to their high melting point, thermal stability, and excellent high-temperature strength.

[0003] However, most of the existing refractory multi-principal alloys are mainly composed of elements such as Nb, Mo, Ta, W, Ti, and Zr, which are difficult to form a dense oxide film at high temperatures and thus exhibit poor high-temperature oxidation resistance.

[0004] Therefore, it is necessary to provide a high-strength and high-oxidation-resistant refractory high-entropy alloy and a preparation method thereof, and to obtain a refractory high-entropy alloy with high strength and high oxidation resistance through reasonable alloy composition design combined with a suitable preparation method. Summary of the invention

[0005] In order to overcome the problems in the background technology, the present invention adopts a reasonable alloy composition ratio. On the one hand, the types of alloy constituent elements are relatively small. At the same time, in the composition of alloy elements, except for Pt, the rest are not precious metals, which effectively reduces the alloy manufacturing cost; on the other hand, the alloy can not only form an oxide layer, effectively preventing the alloy from oxidizing and volatilizing, but also effectively preventing oxygen and nitrogen from penetrating the oxide layer and diffusing inward, thereby significantly improving the high-temperature oxidation resistance of the alloy, so that the alloy has both high strength and good high-temperature oxidation resistance. Combined with the preparation method, the alloy is more uniform after smelting, which is conducive to improving the performance of castings made of the alloy.

[0006] In order to achieve the above object, the present invention is implemented by the following technical solutions:

[0007] On the one hand, the present invention provides a high-strength and high-oxidation-resistant refractory high-entropy alloy, the chemical composition of which is expressed as Pt x CrTaTi, the molar ratio of the component elements in the alloy is Pt:Cr:Ta:Ti=x:1:1:1, where x=0.1~1.

[0008] Another aspect of the present invention provides a method for preparing the above alloy, the preparation method comprising the following steps:

[0009] (1) Pretreatment: remove the surface oxide layer of the elemental metals Pt, Cr, Ta, and Ti, first perform ultrasonic cleaning on the elemental metals, then dry the elemental metals, then perform acid pickling after drying, then perform ultrasonic cleaning on the elemental metals again, and finally wash the elemental metals again to obtain clean elemental metals after drying;

[0010] (2) Vacuum arc melting: weigh the single metals according to the molar ratio of the refractory high entropy alloy elements, and place them in a water-cooled copper mold crucible in the order of Cr, Ta, Ti, and Pt from bottom to top. Vacuum arc melt the single metals in an argon environment. During the melting process, the alloy is turned over and melted at least 5 times. After melting, cool it to obtain an alloy ingot.

[0011] Preferably, the purity of the single metals Pt, Cr, Ta and Ti is 99.99%.

[0012] Preferably, in step (1), anhydrous ethanol is used as the cleaning liquid in the first ultrasonic cleaning, and the cleaning time is 10-15 minutes.

[0013] Preferably, in step (1), the drying temperature is 100° C. and the drying time is 2 h.

[0014] Preferably, in step (1), hydrofluoric acid is used for pickling, and the pickling time is 9-15 minutes.

[0015] Preferably, in step (1), the second ultrasonic cleaning uses clean water as the cleaning liquid, and the clean water is replaced after each cleaning for 9-15 minutes, and the cleaning is repeated for more than 5 times.

[0016] Preferably, in step (1), anhydrous ethanol is used for washing at the end, and the washing time is 10 minutes.

[0017] Preferably, in step (2), the smelting environment is first evacuated to a vacuum and then filled with argon to 0.04-0.05 MPa. At the beginning of smelting, the arc current is first adjusted to 50-100 A. After Pt and Ti are completely melted, the arc current is adjusted to 150-220 A and smelting is continued. The steel is turned over after smelting for at least 5 minutes.

[0018] Preferably, in the step (2), when the alloy is turned over for the first time, it is placed at the edge of the water-cooled copper mold crucible for smelting. When the alloy is turned over each time thereafter, it is placed at the edge of the water-cooled copper mold crucible for smelting. When the alloy is turned over for the last time, it is placed at the center of the water-cooled copper mold crucible for smelting.

[0019] Beneficial effects of the present invention:

[0020] 1. The present invention reasonably designs the alloy composition to form an oxide layer on the alloy, which has a blocking effect on the oxidation and volatilization of elements, and effectively prevents oxygen and nitrogen from penetrating the oxide layer and diffusing inward, thereby significantly improving the high-temperature oxidation resistance of the alloy.

[0021] 2. The present invention reasonably designs the alloy composition so that the alloy has excellent high-temperature oxidation resistance and a strength of 2559 MPa, and the alloy also has relatively high strength.

[0022] 3. Among the alloy components of the present invention, the melting point of Pt metal is 1768.3°C, the melting point of Cr metal is 1907°C, the melting point of Ta metal is 3017°C, and the melting point of Ti metal is 1668°C. The melting points of the metals are quite different, especially the melting point of Ta metal is relatively high. During the smelting process, it is easy for low-melting-point elements to melt while high-melting-point elements cannot be completely and evenly melted in the molten alloy. By placing the alloy on the edge of a water-cooled copper mold crucible for smelting, the melted alloy gradually flows along the side wall of the crucible to the center of the water-cooled copper mold crucible, and the unmelted alloy temporarily stays at the edge of the crucible. Then, by intensively melting the unmelted alloy staying at the edge of the crucible, the molten alloy is made more uniform, thereby making the final alloy ingot more uniform and reducing the defects of the alloy ingot.

[0023] 4. The alloy of the present invention has fewer types of constituent elements, and among the constituent elements, only Pt is a precious metal. Precious metals are considered to be precious metals because of their relatively high prices in the financial market. Therefore, the alloy of the present invention has fewer types of constituent elements, and reducing the types of precious metals in the constituent elements is beneficial to reducing the alloy manufacturing cost and facilitating the industrial production and application of the alloy. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a scanning electron microscope (SEM) image of the refractory high entropy alloy of Example 1 of the present invention;

[0025] Figure 2 This is a scanning electron microscope (SEM) image of the refractory high entropy alloy of Example 2 of the present invention;

[0026] Figure 3 This is a scanning electron microscope (SEM) image of the refractory high entropy alloy of Example 3 of the present invention;

[0027] Figure 4 This is a scanning electron microscope (SEM) image of the refractory high entropy alloy of comparative example 1 of the present invention.

[0028] Figure 5 The room temperature compressive stress-strain curves of the alloys of Examples 1, 2, 3 and Comparative Example 1 of the present invention;

[0029] Figure 6 The oxidation curves of the alloys of Examples 1, 2, 3 and Comparative Example 1 of the present invention in a high temperature environment of 1200° C.

[0030] Figure 7 This is a physical picture of the refractory high entropy alloy of the embodiment of the present invention and the comparative example 1 after being oxidized in a high temperature environment of 1200° C. for 12 hours;

[0031] Figure 8 The actual pictures of the alloy ingots of Example 3 and Comparative Example 2 of the present invention;

[0032] Fig. 9 This is a schematic diagram of the alloy being placed on the edge of a crucible during the alloy smelting process of the present invention;

[0033] Fig.10 This is a physical picture of the refractory high entropy alloy of comparative example 4 of the present invention being oxidized in a high temperature environment of 1200°C for 12 hours. DETAILED DESCRIPTION

[0034] The present invention is further described in detail below in conjunction with specific embodiments.

[0035] All chemical reagents not specifically described in the examples and comparative examples of the present invention were commercially available analytically pure reagents for the experiments.

[0036] Example 1

[0037] This embodiment prepares a refractory high entropy alloy by the following method:

[0038] (1) Take metal blocks of Pt, Cr, Ta and Ti with a purity greater than 99.99%, perform mechanical rough grinding on the four metal blocks in turn to remove the oxide layer on the surface of the metal blocks, then perform ultrasonic cleaning on the metal blocks with anhydrous ethanol for 10 minutes, then dry the metal blocks at 100°C for 2 hours, and after drying, use hydrofluoric acid to pickle the metal blocks for 9 minutes. After pickling, use clean water ultrasonic cleaning on the metal blocks, each cleaning for 9 minutes, repeat the cleaning 6 times, and then use anhydrous ethanol to clean the metal blocks for a total of 10 minutes, and then dry the metal blocks at 100°C for 2 hours for standby use.

[0039] (2) Four metals are taken respectively according to the molar ratio of Pt, Cr, Ta and Ti being Pt:Cr:Ta:Ti=0.1:1:1:1, and then Cr, Ta, Ti and Pt metals are placed in a water-cooled copper mold crucible from bottom to top to reduce the volatilization of the alloy during the smelting process. At the same time, a titanium alloy ingot is placed in the crucible next to it (before starting to smelt the refractory high entropy alloy, the titanium alloy ingot is first melted under the condition of an arc current of 30-80A to absorb the remaining oxygen and nitrogen in the furnace chamber), the furnace door is closed, and the power supply, water cooling cycle and vacuum system are turned on; first, the smelting environment is evacuated to 5MPa with a mechanical pump, and then the smelting environment is evacuated to 2×10-3 After the melting of the titanium alloy ingot, the silver arc current was adjusted to 50A to start the high entropy alloy melting. After the Pt and Ti were melted, the arc current was adjusted to 80A. After melting for at least 5 minutes, the melting was completed. At this time, the alloy ingot was turned over and placed on the edge of the water-cooled copper crucible (such as Fig. 9 As shown), continue to melt it so that it flows to the middle of the water-cooled copper crucible, and complete another melting, and so on. After each melting, turn it over and place the alloy ingot on the edge of the crucible. Turn it over and melt it at least 5 times to ensure the uniformity of chemical composition. During the last melting, place the alloy ingot in the middle of the water-cooled copper crucible. After the melting is completed, close the melting furnace, end the melting, and after cooling, take out the alloy ingot to obtain an alloy ingot with uniform composition.

[0040] The microstructure of the alloy ingot prepared in this example was analyzed. Figure 1 As shown, through Figure 1 It can be seen that the alloy ingot presents an obvious two-phase dendritic structure, and the second phase is mainly distributed at the boundary of the phases and is evenly distributed.

[0041] The mechanical properties of the alloy ingot prepared in this example were analyzed. Figure 5 As shown, through Figure 5 It can be seen that the room temperature compressive limit strength of the alloy in this embodiment is 1888 MPa.

[0042] The oxidation performance of the alloy ingot prepared in this example was tested at 1200°C. The results are as follows: Figure 6 As shown, through Figure 6 It can be seen that the alloy in this example has a weight increase of 8.26 mg / cm after oxidation at 1200°C for 12 h. 2 .

[0043] The alloy ingot prepared in this example is oxidized at 1200°C for 12 hours. Figure 7 As shown. Figure 7 It can be seen that the surface of the alloy ingot prepared in this embodiment has no defects and presents a darker color, which means that the alloy ingot prepared in this embodiment forms a dense oxide layer, which not only effectively oxidizes and volatilizes the elements, but also effectively prevents oxygen and nitrogen from penetrating the oxide layer and diffusing inward, thereby making the alloy have excellent high-temperature oxidation resistance.

[0044] Example 2

[0045] This embodiment prepares a refractory high entropy alloy by the following method:

[0046] (1) Take metal blocks of Pt, Cr, Ta and Ti with a purity greater than 99.99%, perform mechanical rough grinding on the four metal blocks in turn to remove the oxide layer on the surface of the metal blocks, then perform ultrasonic cleaning on the metal blocks with anhydrous ethanol for 12 minutes, then dry the metal blocks at 100°C for 2 hours, and after drying, use hydrofluoric acid to pickle the metal blocks for 13 minutes. After pickling, use clean water to ultrasonically clean the metal blocks, each time for 12 minutes, repeat the cleaning 7 times, and then use anhydrous ethanol to clean the metal blocks for a total of 10 minutes, and then dry the metal blocks at 100°C for 2 hours for standby use.

[0047] (2) Four metals are taken respectively according to the molar ratio of Pt, Cr, Ta and Ti being Pt:Cr:Ta:Ti=0.25:1:1:1, and then Cr, Ta, Ti and Pt metals are placed in a water-cooled copper mold crucible from bottom to top to reduce the volatilization of the alloy during the smelting process. At the same time, a titanium alloy ingot is placed in the crucible next to it (before starting to smelt the refractory high entropy alloy, the titanium alloy ingot is first melted to absorb the remaining oxygen and nitrogen in the furnace chamber), the furnace door is closed, and the power supply, water cooling cycle and vacuum system are turned on; the smelting environment is first evacuated to 5 MPa using a mechanical pump, and then the smelting environment is evacuated to 2×10 -3 After Pa, argon is filled to 0.045MPa, the arc striking current is adjusted to 50A, and the arc striking switch is turned on to melt the titanium alloy ingot; after the titanium alloy ingot is melted, the silver arc current is adjusted to 80A, and the high entropy alloy smelting is started. After Pt and Ti are melted, the arc striking current is adjusted to 180A. After smelting for at least 5 minutes, a smelting is completed. At this time, the alloy ingot is turned over and placed on the edge of the water-cooled copper crucible. The smelting is continued to make it flow to the middle of the water-cooled copper crucible, and another smelting is completed. By analogy, each time a smelting is completed, the alloy ingot is turned over and placed on the edge of the crucible. It is turned over and melted at least 5 times to ensure the uniformity of the chemical composition; during the last smelting, the alloy ingot is placed in the middle of the water-cooled copper crucible. After the smelting is completed, the smelting furnace is closed to end the smelting. After cooling is completed, the alloy ingot is taken out to obtain an alloy ingot with uniform composition.

[0048] The microstructure of the alloy ingot prepared in this example was analyzed. Figure 2 As shown, through Figure 2 It can be seen that the structure of the alloy ingot presents an obvious three-phase dendritic structure. At the same time, compared with Example 1, the phase distinction is more obvious, and a black and white phase appears.

[0049] The mechanical properties of the alloy ingot prepared in this example were analyzed. Figure 5 As shown, through Figure 5It can be seen that the room temperature compressive limit strength of the alloy ingot of this embodiment is 1987 MPa, which is higher than that of the alloy ingot prepared in Example 1.

[0050] The oxidation performance of the alloy ingot prepared in this example was tested at 1200°C. The results are as follows: Figure 6 As shown, through Figure 6 It can be seen that the alloy in this embodiment has a weight increase of 6.91 mg / cm after oxidation at 1200°C for 12 h. 2 .

[0051] The alloy ingot prepared in this example is oxidized at 1200°C for 12 hours. Figure 7 As shown. Figure 7 It can be seen that the alloy ingot prepared in this embodiment is similar to that in Embodiment 1 and has similar properties.

[0052] Example 3

[0053] This embodiment prepares a refractory high entropy alloy by the following method:

[0054] (1) Take metal blocks of Pt, Cr, Ta and Ti with a purity greater than 99.99%, perform mechanical rough grinding on the four metal blocks in turn to remove the oxide layer on the surface of the metal blocks, then perform ultrasonic cleaning on the metal blocks with anhydrous ethanol for 15 minutes, then dry the metal blocks at 100°C for 2 hours, and after drying, use hydrofluoric acid to pickle the metal blocks for 15 minutes. After pickling, use clean water to ultrasonically clean the metal blocks, each time for 15 minutes, repeat the cleaning 8 times, and then use anhydrous ethanol to clean the metal blocks for a total of 10 minutes, and then dry the metal blocks at 100°C for 2 hours for use.

[0055] (2) Take four metals according to the molar ratio of Pt, Cr, Ta and Ti of Pt:Cr:Ta:Ti=1:1:1:1, and then place the Cr, Ta, Ti and Pt metals in a water-cooled copper mold crucible from bottom to top to reduce the volatilization of the alloy during the smelting process. At the same time, place a titanium alloy ingot in the crucible next to it (before starting to smelt the refractory high-entropy alloy, first melt the titanium alloy ingot to absorb the remaining oxygen and nitrogen in the furnace chamber), close the furnace door, turn on the power supply, water cooling cycle and vacuum system; first use a mechanical pump to evacuate the melting environment to 5MPa, and then use a molecular pump to evacuate the melting environment to 2×10 -3After Pa, argon is filled to 0.05MPa, the arc current is adjusted to 80A, and the arc switch is turned on to melt the titanium alloy ingot; after the titanium alloy ingot is melted, the silver arc current is adjusted to 100A, and the high entropy alloy smelting is started. After Pt and Ti are melted, the arc current is adjusted to 220A. After smelting for at least 5 minutes, a smelting is completed. At this time, the alloy ingot is turned over and placed on the edge of the water-cooled copper crucible. The smelting is continued to make it flow to the middle of the water-cooled copper crucible, and another smelting is completed. By analogy, each time a smelting is completed, the alloy ingot is turned over and placed on the edge of the crucible. It is turned over and melted at least 5 times to ensure the uniformity of the chemical composition; during the last smelting, the alloy ingot is placed in the middle of the water-cooled copper crucible. After the smelting is completed, the smelting furnace is closed to end the smelting. After cooling is completed, the alloy ingot is taken out to obtain an alloy ingot with uniform composition.

[0056] The microstructure of the alloy ingot prepared in this example was analyzed. Figure 3 As shown, through Figure 3 It can be seen that the structure of the alloy ingot presents an obvious three-phase dendritic structure. Compared with Example 2, the distinction between the phases of the alloy ingot in this example is more obvious.

[0057] The mechanical properties of the alloy ingot prepared in this example were analyzed. Figure 5 As shown, through Figure 5 It can be seen that the room temperature compressive limit strength of the alloy ingot of this embodiment is 2559 MPa.

[0058] The oxidation performance of the alloy ingot prepared in this example was tested, and the results are as follows: Figure 6 As shown, through Figure 6 It can be seen that the alloy in this example has a weight increase of 3.46 mg / cm after oxidation at 1200°C for 12 h. 2 .

[0059] The alloy ingot prepared in this example is oxidized at 1200°C for 12 hours. Figure 7 As shown. Figure 7 It can be seen that the alloy ingot prepared in this embodiment is similar to that in Embodiment 1 and has similar properties.

[0060] The alloy component prepared in this embodiment is as follows Figure 8 shown.

[0061] Comparative Example 1

[0062] In this comparative example, the alloy ingot was prepared by the same method as in the example, except that no Pt element was added to the alloy, and the molar ratio of the alloy components was Cr:Ta:Ti=1:1:1.

[0063] The alloy ingot prepared in this comparative example was subjected to microstructural analysis, and the results are as follows: Figure 4 As shown, through Figure 4 It can be seen that the microstructure of the alloy of Comparative Example 1 also presents a two-phase dendritic structure, and its microstructure is similar to that of Example 1. Therefore, its compressive limit strength is closer to that of Example 1, but the amount of its second phase is small and the distribution uniformity is poor. Therefore, its compressive limit strength is lower than that of Example 1. Since it is not a three-phase dendritic structure, its strength is significantly lower than that of the alloys of Examples 2 and 3.

[0064] The mechanical properties of the alloy ingot prepared in this comparative example were analyzed, and the results are as follows: Figure 5 As shown, through Figure 5 It can be seen that the room temperature compressive limit strength of the alloy ingot of this embodiment is 1835 MPa.

[0065] The oxidation performance of the alloy ingot prepared in this comparative example was tested, and the results are as follows: Figure 6 As shown, through Figure 6 It can be seen that the alloy in this embodiment has a weight increase of 18.46 mg / cm after oxidation at 1200°C for 12 h. 2 .

[0066] The alloy ingot prepared in this comparative example is oxidized at 1200°C for 12 hours. Figure 7 As shown. Figure 7 It can be seen that after oxidation, obvious defects appear on the surface of the alloy ingot of this comparative example, and no oxide layer is formed, so its oxidation resistance is poor.

[0067] Comparative Example 2

[0068] This comparative example adopts the same method as the embodiment to prepare the alloy ingot, except that during the overturning smelting process, the alloy ingot is placed in a crucible for smelting.

[0069] The alloy ingots prepared in this comparative example and Example 3 were observed after wire cutting. Figure 8 As shown, the alloy ingot prepared in this comparative example has obvious unevenness compared with the alloy ingot prepared in Example 3. During the use of the alloy component, the mechanical properties and oxidation resistance of the uneven part are poor, that is, the alloy is very easy to be broken at the uneven part, thereby causing damage to the alloy component. Therefore, it is necessary to avoid defects such as unevenness during the alloy smelting process as much as possible.

[0070] Comparative Example 3

[0071] The alloy ingot was prepared in the present comparative example by the same method as in the embodiment, except that the molar ratio of the alloy components in the present comparative example was: W:Nb:Zr:Ti=1:1:1:1.

[0072] The alloy ingots of this comparative example are as follows before and after oxidation: Fig.10 As shown, through Fig.10 It can be seen that the alloy ingot prepared in this comparative example is almost completely destroyed after being oxidized at 1200°C for 12 hours. Since the alloy ingot in this comparative example hardly forms an oxide film, the alloy ingot in this comparative example has almost no high-temperature oxidation resistance.

[0073] The alloy ingot prepared by the present invention has a maximum compressive ultimate strength of 2559 MPa, which is significantly increased compared with comparative example 1 (1835 MPa). The alloy ingot prepared by the present invention has higher strength.

[0074] The alloy ingot prepared by the present invention has a weight gain of only 3.46 mg / cm after being oxidized at 1200°C for 12 hours. 2 The less the alloy weight gain, the better its anti-oxidation performance. The higher the temperature, the easier the alloy is oxidized, that is, the higher the temperature, the greater the difficulty of the alloy's anti-oxidation. At the same time, the increase in temperature and the difficulty of the alloy's anti-oxidation do not increase linearly, but the increase in temperature will greatly increase the difficulty of the alloy's anti-oxidation. Therefore, the alloy prepared by the present invention still has excellent anti-oxidation performance under high temperature conditions and in an environment with greater anti-oxidation difficulty.

[0075] In summary, the present invention, through reasonable alloy composition design and combined with a suitable preparation method, obtains an alloy with high strength, excellent high-temperature oxidation resistance and good uniformity. The alloy has good performance and can meet higher application requirements.

[0076] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made in form and details without departing from the scope defined by the claims of the present invention.

Claims

1. A high-strength and high-oxidation-resistant refractory high-entropy alloy, characterized in that: The alloy chemical composition expression is Pt x CrTaTi, the molar ratio of the component elements in the alloy is Pt:Cr:Ta:Ti=x:1:1:1, where x=0.1~1.

2. A method for preparing a high-strength and high-oxidation-resistant refractory high-entropy alloy according to claim 1, characterized in that: The preparation method comprises the following steps: (1) Pretreatment: remove the surface oxide layer of the elemental metals Pt, Cr, Ta, and Ti, first perform ultrasonic cleaning on the elemental metals, then dry the elemental metals, then perform acid pickling after drying, then perform ultrasonic cleaning on the elemental metals again, and finally wash the elemental metals again to obtain clean elemental metals after drying; (2) Vacuum arc melting: weigh the single metals according to the molar ratio of the refractory high entropy alloy elements, and place them in a water-cooled copper mold crucible in the order of Cr, Ta, Ti, and Pt from bottom to top. Vacuum arc melt the single metals in an argon environment. During the melting process, the alloy is turned over and melted at least 5 times. After melting, cool it to obtain an alloy ingot.

3. A method for preparing a refractory high entropy alloy according to claim 2, characterized in that: The purity of the single metals Pt, Cr, Ta and Ti is 99.99%.

4. A method for preparing a refractory high entropy alloy according to claim 2, characterized in that: In the step (1), the first ultrasonic cleaning uses anhydrous ethanol as a cleaning liquid, and the cleaning time is 10-15 minutes.

5. A method for preparing a refractory high entropy alloy according to claim 2, characterized in that: In the step (1), the drying temperature is 100° C. and the drying time is 2 h.

6. A method for preparing a refractory high entropy alloy according to claim 2, characterized in that: In the step (1), hydrofluoric acid is used for pickling, and the pickling time is 9-15 minutes.

7. A method for preparing a refractory high entropy alloy according to claim 2, characterized in that: In the step (1), the second ultrasonic cleaning uses clean water as the cleaning liquid. After each cleaning for 9-15 minutes, the clean water is replaced and the cleaning is repeated for more than 5 times.

8. A method for preparing a refractory high entropy alloy according to claim 2, characterized in that: In the step (1), anhydrous ethanol is used for washing at last, and the washing time is 10 minutes.

9. A method for preparing a refractory high entropy alloy according to claim 2, characterized in that: In the step (2), the smelting environment is first evacuated to a vacuum, and then filled with argon to 0.04-0.05 MPa. At the beginning of smelting, the arc current is first adjusted to 50-100 A. After Pt and Ti are completely melted, the arc current is adjusted to 150-220 A and smelting is continued. After smelting for at least 5 minutes, the surface is turned over.

10. A method for preparing a refractory high entropy alloy according to claim 2, characterized in that: In the step (2), when the alloy is turned over for the first time, it is placed at the edge of the water-cooled copper mold crucible for smelting. When the alloy is turned over each time thereafter, it is placed at the edge of the water-cooled copper mold crucible for smelting. When the alloy is turned over for the last time, it is placed at the center of the water-cooled copper mold crucible for smelting.