Laser cladding wear-resistant coating for titanium alloy surface and preparation method of laser cladding wear-resistant coating

By using the combination of NiCoCrAlYW, NbN, PTFE and BaF2 powders, laser cladding technology is used to form a wear-resistant coating on the surface of the titanium alloy, which solves the problems of low hardness and poor wear resistance of the titanium alloy, and achieves uniformity and high efficiency of the coating Performance, suitable for different temperature environments.

CN119082584APending Publication Date: 2024-12-06ZHENGZHOU COAL MASCH GREEN MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411304592.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Titanium alloy has low hardness and poor wear resistance. The uneven cladding of high-melting and low-melting materials in the existing laser cladding process leads to the inability to fully meet expectations, which limits the application of titanium alloy in aerospace and other fields.

Method used

Laser cladding wear-resistant coating was prepared by 60%-70% NiCoCrAlYW powder, 20%-25% NbN, 10%-13% PTFE and 1%-3% BaF2 powder. After mixing and drying, the mixture was performed by ball milling. , a composite powder coating is formed on the surface of the titanium alloy by coaxial powder feeding, and after the coating is cooled, PTFE powder is sprayed with a high-speed spray gun to ensure uniform dispersion.

Benefits of technology

The hardness, wear resistance and corrosion resistance of the surface of titanium alloy is significantly improved, and the problem of uneven material cladding in thermal spraying and traditional laser cladding processes is overcome, achieving excellent wear resistance under different temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082584A_ABST
    Figure CN119082584A_ABST
Patent Text Reader

Abstract

The invention relates to preparation of a surface modification and wear-resistant coating, in particular to the field of titanium alloy surface laser cladding strengthening. Different lubricant raw materials are added in the preparation process of the coating, so that the obtained cladding coating has higher hardness and good corrosion resistance and wear resistance, also realizes a low friction coefficient in a full temperature range, and has excellent friction reduction and wear resistance. And the PTFE raw material is deposited in a high-speed spraying manner, so that high-temperature decomposition in the laser cladding process is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to surface modification and preparation of wear-resistant coating, and in particular to the field of laser cladding strengthening of titanium alloy surface. Background Art

[0002] In the prior art, iron-based, nickel-based, cobalt-based alloys are usually used as the main powder materials, and hard particles and lubricating materials are added to prepare coating materials, thereby improving the surface wear resistance, corrosion resistance, lubrication performance, etc. of the substrate workpiece. Common coating preparation methods include thermal spraying, cold spraying, physical vapor deposition, laser cladding, etc., and the most commonly used preparation methods for strengthening coatings are thermal spraying, cold spraying and laser cladding. The thermal spraying method can be used for spraying and depositing a variety of materials such as metals, ceramics, and polymers, and has a wide range of application scenarios. However, during the thermal spraying process, the powder particles are ejected at high speed onto the substrate surface, and most of the obtained coatings are layered structures. The powder particles ejected from the rear layer impact the coating of the front layer at high speed, resulting in the overall thermal spray coating showing low density, high porosity and surface roughness, which directly affects the wear resistance and corrosion resistance of the coating. Cold spraying also has the problems of preparing coatings by high-speed spraying of powder particles, and cold spraying is mainly used for spraying powder particles with low melting points, and is not suitable for spraying high melting point powder materials, which also limits the scope of application of cold spraying.

[0003] Laser cladding is another commonly used method for preparing strengthening coatings. The coating prepared by laser cladding is metallurgically bonded to the substrate, and the coating is dense, which helps to improve the wear resistance and corrosion resistance of the coating. The laser used in laser cladding has the characteristics of high energy density and high temperature, and can be used for spraying high-melting-point metals and even ceramic materials. However, due to this characteristic, the laser cladding deposition method is not suitable for the deposition of low-melting-point powder materials. For different materials with very different melting points in the cladding powder material, due to the large difference in their melting points, the use of the same energy density laser is likely to cause the high-melting-point material to not be completely melted or the low-melting-point material to decompose. This technical problem also limits the use of laser cladding. This technical problem also exists in the thermal spray process. In order to overcome this technical defect, the existing technology pre-places the low-melting-point cladding material in the lower layer and the high-melting-point material in the upper layer, and then performs laser cladding treatment. This method can solve the problem of simultaneous cladding of high-melting-point materials and low-melting-point materials to a certain extent. However, due to the layered arrangement of the two, the prepared cladding layer is uneven, and the lower layer material cannot completely enter the upper layer, resulting in the cladding layer performance not being able to fully achieve the expected effect.

[0004] As an emerging metal material, titanium alloy is widely used in aerospace, marine shipbuilding, automobile manufacturing and other fields due to its low density, good corrosion resistance and excellent thermal stability. However, titanium alloy has low hardness and relatively poor wear resistance, which greatly shortens its service life and limits its application.

[0005] Therefore, a solution is needed to solve the technical problems existing in the prior art. In view of this, the present invention proposes a method for preparing a wear-resistant coating on the surface of a laser-clad titanium alloy to solve the low hardness and poor wear resistance of the titanium alloy and the technical problems existing in the existing laser cladding process. The method has the characteristics of low cost, strong operability, and excellent coating performance, etc., and has attracted widespread attention. Summary of the invention

[0006] The present invention provides a laser cladding wear-resistant coating for titanium alloy surface, a preparation method and titanium alloy coated with the wear-resistant coating, which can at least solve some problems existing in the prior art.

[0007] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions: A laser cladding wear-resistant coating for a titanium alloy surface, wherein the wear-resistant coating is prepared from powder raw materials in the following mass percentages: 60%-70% NiCoCrAlYW, 20%-25% NbN, 10%-13% PTFE and 1%-3% BaF2.

[0008] As a preferred solution of the laser cladding wear-resistant coating for titanium alloy surface described in the present invention, the mass percentage of each component in the NiCoCrAlYW powder is: Co: 28-30%, Cr: 20-25%, Al: 5-7%, Y: 0.5-1.0%, W: 5-10%, and the balance is Ni.

[0009] As a preferred solution of the laser cladding wear-resistant coating for titanium alloy surface described in the present invention, the particle size of NiCoCrAlYW powder is 100-200μm, the particle size of NbN powder is 50-104μm, the particle size of PTFE powder is 1.0-5.0μm, and the particle size of BaF2 powder is 50-100μm.

[0010] To solve the above technical problem, according to another aspect of the present invention, the present invention provides the following technical solution: A method for preparing a laser cladding wear-resistant coating on a titanium alloy surface comprises the following steps: Step 1: Weigh NiCoCrAlYW powder, NbN powder, PTFE powder and BaF2 powder raw materials required for preparing the coating according to a predetermined mass ratio; Step 2: ball milling the NiCoCrAlYW powder, NbN powder and BaF2 powder to obtain a composite powder; Step 3: Dry the mixed composite powder and PTFE powder separately, and perform surface pretreatment on the TC4 titanium alloy workpiece to be clad; Step 4: Perform laser cladding on the workpiece to be clad after surface pretreatment to form a composite powder coating on the surface of the workpiece to be clad. The laser cladding of the composite powder adopts a coaxial powder feeding method for cladding deposition. The deposition of PTFE powder adopts a high-speed spray gun powder feeding method. The high-speed spray gun and the laser cladding nozzle maintain a fixed distance. After the composite powder cladding layer is cooled to a certain temperature, the high-speed spray gun sprays the PTFE powder into the composite powder cladding layer at a high speed; Step 5: Clean the welding slag and impurities on the coating surface to obtain the laser cladding workpiece.

[0011] As a preferred embodiment of the method for preparing a laser cladding wear-resistant coating on a titanium alloy surface described in the present invention, wherein: in step 2, the NiCoCrAlYW powder, NbN powder and BaF2 powder are ball milled by planetary ball milling, the ball milling rate is 300-500 rpm, the ball milling time is 1-3h, and the ball-to-material mass ratio is 1:(2-4).

[0012] As a preferred embodiment of the method for preparing a laser cladding wear-resistant coating on a titanium alloy surface described in the present invention, the drying parameters of the composite powder and the PTFE powder in step 3 are both drying at 100-200° C. for 1-2 hours.

[0013] As a preferred embodiment of the method for preparing a laser cladding wear-resistant coating on a titanium alloy surface described in the present invention, the surface pretreatment in step 3 is as follows: the workpiece to be clad is cut to the required size by wire cutting, the surface of the workpiece to be clad is polished with 80-200 mesh tungsten carbide sandpaper, and then cleaned and dried.

[0014] As a preferred embodiment of the method for preparing a laser cladding wear-resistant coating on the surface of a titanium alloy described in the present invention, the cladding process parameters of the composite powder in step 4 are: laser power 1200-1500W, laser scanning speed 5-8mm / s, powder feeding speed 12-16g / min, overlap rate 30-45%, spot diameter 3-5mm, argon protection is adopted during the cladding process, the argon flow rate is 10-16L / min, the cladding length of each laser cladding pass is 120-150mm, and a total of 20-40 passes are clad.

[0015] As a preferred embodiment of the method for preparing a laser cladding wear-resistant coating on a titanium alloy surface described in the present invention, the thickness of the laser cladding wear-resistant coating is 0.8-1.2 mm, and no cracks are found on the surface of the laser cladding wear-resistant coating by DPT inspection.

[0016] A titanium alloy, wherein the surface of the titanium alloy comprises a wear-resistant coating prepared by any of the preparation methods described above.

[0017] The beneficial effects of the present invention are as follows: 1. The laser cladding wear-resistant coating for titanium alloy surface provided by the present invention and its preparation method use NiCoCrAlYW powder with high hardness, high wear resistance and corrosion resistance in the cladding raw material powder, and additionally add high hardness and high wear resistance ceramic powder NbN, as well as solid lubricating materials PTFE and BaF2. The prepared cladding coating modifies the titanium alloy surface, thereby improving the hardness, wear resistance and corrosion resistance of the titanium alloy.

[0018] 2. The laser cladding wear-resistant coating for titanium alloy surface provided by the present invention and its preparation method overcome the technical defects of thermal spraying process and traditional laser cladding process that powder materials with large differences cannot be melted and formed at the same time and coatings with expected performance cannot be prepared. The present invention does not mix and clad the low-melting-point PTFE powder with other powder materials, nor does it layer the low-melting-point PTFE powder with other powder materials. Instead, the PTFE powder material is sprayed at high speed after the other powder materials are clad and formed, which not only avoids the PTFE powder from being melted and decomposed by the high-temperature laser beam, but also ensures that the PTFE powder can be evenly dispersed within a certain depth on the surface of the cladding layer to achieve lubrication performance.

[0019] 3. The cladding powder material provided by the present invention contains different types of lubricating materials. The W element in the NiCoCrAlYW powder combines with the oxygen element in the air to form tungsten trioxide when the wear-resistant coating is used under temperature conditions above 1000°C. Tungsten trioxide can reduce the friction coefficient of the wear-resistant coating under high temperature conditions and play a role in lubrication and friction reduction under high temperature conditions. BaF2 has a lower friction coefficient under medium temperature conditions of 600-1000°C, while PTFE can play a lubricating role in low temperature environments below 500°C. Therefore, the wear-resistant coating provided by the present invention has good friction reduction and lubrication properties in low temperature, medium temperature and high temperature full temperature range environments, so that the titanium alloy has excellent wear resistance under different working conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0021] Figure 1 The metallographic structure of the NiCoCrAlYW-NbN-PTFE-BaF2 wear-resistant coating prepared in Example 1 of the present invention; Figure 2 This is the SEM scanning structure of the NiCoCrAlYW-NbN-PTFE-BaF2 wear-resistant coating prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0022] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] It should be noted that if the embodiments of the present invention involve directional indications (such as up, down, left, right, front, back...), the directional indications are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.

[0024] In addition, if there are descriptions involving "first", "second", etc. in the embodiments of the present invention, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or suggesting their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0025] The invention provides a laser cladding wear-resistant coating for titanium alloy surface, a preparation method and titanium alloy coated with the wear-resistant coating, which can improve the surface hardness, corrosion resistance and wear resistance of the titanium alloy.

[0026] A laser cladding wear-resistant coating for a titanium alloy surface, wherein the wear-resistant coating is prepared from powder raw materials in the following mass percentages: 60%-70% NiCoCrAlYW, 20%-25% NbN, 10%-13% PTFE and 1%-3% BaF2.

[0027] Preferably, the mass percentages of the components in the NiCoCrAlYW powder are: Co: 28-30%, Cr: 20-25%, Al: 5-7%, Y: 0.5-1.0%, W: 5-10%, and the balance Ni.

[0028] As the main alloy element, Ni plays a key role in alloy materials. Ni can improve the strength of the alloy and is crucial to improving the mechanical properties of the material. Ni can also improve the corrosion resistance, wear resistance and oxidation resistance of the alloy, which is particularly important for substrates used in corrosive environments and high temperature or high wear environments. The content of Ni can be determined by the remainder when other elements in the alloy are determined.

[0029] The Al element is mainly used to improve the oxidation resistance and heat resistance of the alloy. The content of the Al element used in the present invention is appropriately reduced on the basis of the prior art. This is mainly because the Al element in the alloy and the Ti element in the matrix will produce brittle intermetallic compounds, which may have an adverse effect on the mechanical properties of the coating.

[0030] In addition to enhancing the strength and hardness of the alloy, the Co element mainly provides the alloy with corrosion resistance and heat resistance. The content of the Co element is appropriately increased on the basis of the Co element content of the traditional NiCoCrAlY-based alloy to make up for the lack of strength and heat resistance of the titanium alloy and the reduction of the Al element content in the alloy powder to reduce the improvement of the heat resistance of the coating.

[0031] Cr element is beneficial to improve the wear resistance and oxidation resistance of the alloy, and can protect the base material from oxidation corrosion in high temperature environment. The content of Cr element is also appropriately increased on the basis of the Cr element content of the traditional NiCoCrAlY-based alloy to make up for the lack of thermal oxidation resistance of titanium alloy and the reduction of Al element content in alloy powder to reduce the improvement of coating oxidation resistance.

[0032] Y element can improve the structure and performance, and then improve the phase stability in the alloy and the mechanical properties of the coating. W is a high melting point metal element. When it is added to the cladding alloy powder, the resulting wear-resistant coating forms a tungsten trioxide film with lubricating properties in a high temperature wear environment, thereby reducing the wear of the substrate.

[0033] Ceramic particles NbN can further improve coating performance and optimize the wettability of the coating and substrate. Preferably, the particle size of the NiCoCrAlYW powder is 100-200 μm, the particle size of the NbN powder is 50-104 μm, the particle size of the PTFE powder is 1.0-5.0 μm, and the particle size of the BaF2 powder is 50-100 μm.

[0034] A method for preparing a laser cladding wear-resistant coating on a titanium alloy surface comprises the following steps: Step 1: Weigh NiCoCrAlYW powder, NbN powder, PTFE powder and BaF2 powder raw materials required for preparing the coating according to a predetermined mass ratio; Step 2: ball milling the NiCoCrAlYW powder, NbN powder and BaF2 powder to obtain a composite powder; Step 3: Dry the mixed composite powder and PTFE powder separately, and perform surface pretreatment on the TC4 titanium alloy workpiece to be clad; Step 4: Perform laser cladding on the workpiece to be clad after surface pretreatment to form a composite powder coating on the surface of the workpiece to be clad. The laser cladding of the composite powder adopts a coaxial powder feeding method for cladding deposition. The deposition of PTFE powder adopts a high-speed spray gun powder feeding method. The high-speed spray gun and the laser cladding nozzle maintain a fixed distance. After the composite powder cladding layer is cooled to a certain temperature, the high-speed spray gun sprays the PTFE powder into the composite powder cladding layer at a high speed; Step 5: Clean the welding slag and impurities on the coating surface to obtain the laser cladding workpiece.

[0035] During the spraying of PTFE powder by a high-speed spray gun, the selection of the distance between the high-speed spray gun and the laser cladding nozzle mainly considers the temperature of the alloy coating in the molten pool, and the standard is that the PTFE does not decompose significantly when it enters the alloy coating. The molten pool temperature should not be too high when the high-speed spray gun is spraying, otherwise the PTFE powder will decompose into other components when it is sprayed into the alloy coating, and it will not play the role of friction reduction and lubrication; the molten pool temperature should not be too low, otherwise the PTFE powder particles cannot enter the alloy coating.

[0036] Preferably, in step 2, the NiCoCrAlYW powder, NbN powder and BaF2 powder are ball milled by planetary ball milling, the ball milling rate is 300-500 rpm, the ball milling time is 1-3h, and the ball-to-material mass ratio is 1:(2-4).

[0037] Preferably, in step 3, the drying parameters of the composite powder and the PTFE powder are both 100-200° C. for 1-2 hours.

[0038] Preferably, the surface pretreatment in step 3 is: cutting the workpiece to be clad to a required size by wire cutting, grinding the surface of the workpiece to be clad with 80-200 mesh tungsten carbide sandpaper, and then cleaning and drying.

[0039] Preferably, the cladding process parameters for the composite powder in step 4 are: laser power 1200-1500W, laser scanning speed 5-8mm / s, powder feeding speed 12-16g / min, overlap rate 30-45%, spot diameter 3-5mm, argon protection is adopted during the cladding process, argon flow rate is 10-16L / min, laser cladding length of each pass is 120-150mm, and a total of 20-40 passes are clad.

[0040] Preferably, the thickness of the laser cladding wear-resistant coating is 0.8-1.2 mm, and no cracks are found on the surface of the laser cladding wear-resistant coating by DPT testing.

[0041] The technical solution of the present invention is further described and explained below in conjunction with specific embodiments.

[0042] Example 1 A method for preparing a laser cladding wear-resistant coating on a titanium alloy surface comprises the following steps: Step 1: Weigh the NiCoCrAlYW powder, NbN powder, PTFE powder and BaF2 powder raw materials required for preparing the coating according to the following mass ratio: 65% NiCoCrAlYW, 20% NbN, 12% PTFE and 3% BaF2. The mass percentage of each component in the NiCoCrAlYW powder is: Co: 28%, Cr: 24%, Al: 6%, Y: 1.0%, W: 8%, and the balance is Ni.

[0043] Step 2: The NiCoCrAlYW powder, NbN powder and BaF2 powder are mixed by planetary ball milling to obtain a composite powder. The ball milling rate is 400 rpm, the ball milling time is 2 h, and the ball-to-material mass ratio is 1:3.

[0044] Step 3: Dry the mixed composite powder and PTFE powder separately, and perform surface pretreatment on the TC4 titanium alloy workpiece to be clad. The drying temperature is 150° C. and the time is 1 h.

[0045] The surface pretreatment method is: cut the workpiece to be clad to the required size by wire cutting, grind the surface of the workpiece with different tungsten carbide sandpapers of 80-200 mesh, and then wash it with deionized water and blow dry it.

[0046] Step 4: Perform laser cladding on the workpiece to be clad after surface pretreatment to form a composite powder coating on the surface of the workpiece to be clad. The laser cladding of the composite powder adopts a coaxial powder feeding method for cladding deposition. The deposition of PTFE powder adopts a high-speed spray gun powder feeding method. The high-speed spray gun and the laser cladding nozzle maintain a fixed distance. After the composite powder cladding layer is cooled to a certain temperature, the high-speed spray gun sprays the PTFE powder into the composite powder cladding layer at a high speed; The cladding process parameters are: laser power 1250W, laser scanning speed 6mm / s, powder feeding speed 16g / min, overlap rate 30%, spot diameter 4mm, argon protection is used during the cladding process, argon flow rate is 12L / min, the cladding length of each laser cladding pass is 150mm, and a total of 30 passes are performed.

[0047] Step 5: Clean the welding slag and impurities on the coating surface to obtain the laser cladding workpiece.

[0048] Comparative Example 1 The preparation method of the wear-resistant coating is the same as the steps of the above-mentioned embodiment 1, except that the powder used for cladding is NiCoCrAlY, which does not contain the W element, and the content of the W element is replaced by the Ni element.

[0049] Comparative Example 2 The preparation method of the wear-resistant coating also adopts the laser cladding method, which has the same cladding powder composition and process parameters as the above-mentioned Example 1. The difference is that the PTFE powder is not sprayed separately at high speed, but the PTFE powder is ball-milled together with other powders, and then clad together to prepare the wear-resistant coating.

[0050] Comparative Example 3 The preparation method of the wear-resistant coating also adopts the laser cladding method, and has the same cladding powder composition and process parameters as the above-mentioned Example 1. The difference is that the PTFE powder is not sprayed separately at high speed, but the PTFE powder and the composite powder are pre-layered separately before laser cladding, with the PTFE powder layer at the bottom and the composite powder layer at the top, and then the same laser cladding parameters are used for cladding to prepare the wear-resistant coating.

[0051] The hardness and wear resistance of the wear-resistant coatings prepared in the above examples and comparative examples were tested. The wear resistance test showed the wear rate (in mm) at three different temperature conditions: low temperature, medium temperature and high temperature. 3 / N·m). The wear rate was tested using a ball-on-disk contact friction and wear tester. The test temperature range was 60℃, 600℃, and 1200℃. The dual material was a tungsten carbide ceramic ball with a diameter of 6mm. The load was 10N, the speed was 300r / min, the friction radius was 5mm, and the running time was 60min.

[0052] The specific test results are shown in the following table.

[0053] The test results of the embodiments and comparative examples are analyzed and compared with the titanium alloy matrix 341HV 0.2 Compared with the hardness of the titanium alloy substrate, the wear-resistant coatings prepared by the above four methods have greatly improved the surface hardness of the titanium alloy substrate. The NiCoCrAlYW alloy material and NbN ceramic material in the coating have played a corresponding role in improving the mechanical properties of the substrate.

[0054] From the wear rate test, the wear-resistant coating material and the wear-resistant coating obtained by the preparation method of the present invention show excellent wear resistance under low temperature, medium temperature and high temperature conditions. In comparison, the W element is not added to the cladding powder material of Example 1, which has little effect on the wear resistance of the wear-resistant coating in low temperature and medium temperature environments. The greater impact is the wear under high temperature conditions. Its wear rate has increased significantly in a friction environment of 1200°C. Due to the co-cladding of PTFE and other raw materials, the wear-resistant coating of Example 2 may cause part of the PTFE to be burned and decomposed during the cladding process, thereby affecting the wear resistance of the wear-resistant coating, especially the wear resistance in a low temperature environment. In the preparation process of the wear-resistant coating of Example 3, PTFE is pre-set in the bottom layer, and there may be a certain amount of burning and decomposition during the cladding process. In addition, the PTFE in the bottom layer cannot be completely transferred to the wear-resistant coating in the cladding pool, especially the surface of the wear-resistant coating, resulting in a certain reduction in the wear resistance of the obtained wear-resistant coating in a low temperature environment. In summary, the wear-resistant coating composition and preparation process of the present invention have a significant effect on improving the wear resistance of the titanium alloy substrate, and can greatly improve the application range of the titanium alloy under different temperature conditions.

[0055] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A laser cladding wear-resistant coating for titanium alloy surface, characterized in that: The wear-resistant coating is prepared from the following powder raw materials in the following mass percentages: 60%-70% NiCoCrAlYW, 20%-25% NbN, 10%-13% PTFE and 1%-3% BaF2.

2. The laser cladding wear-resistant coating for titanium alloy surface according to claim 1, characterized in that: The mass percentages of the components in the NiCoCrAlYW powder are: Co: 28-30%, Cr: 20-25%, Al: 5-7%, Y: 0.5-1.0%, W: 5-10%, and the balance is Ni.

3. The laser cladding wear-resistant coating for titanium alloy surface according to claim 2, characterized in that: The particle size of NiCoCrAlYW powder is 100-200 μm, the particle size of NbN powder is 50-104 μm, the particle size of PTFE powder is 1.0-5.0 μm, and the particle size of BaF2 powder is 50-100 μm.

4. A method for preparing a laser cladding wear-resistant coating for a titanium alloy surface according to any one of claims 1 to 3, comprising the following steps: Step 1: Weigh NiCoCrAlYW powder, NbN powder, PTFE powder and BaF2 powder raw materials required for preparing the coating according to a predetermined mass ratio; Step 2: ball milling the NiCoCrAlYW powder, NbN powder and BaF2 powder to obtain a composite powder; Step 3: Dry the mixed composite powder and PTFE powder separately, and perform surface pretreatment on the TC4 titanium alloy workpiece to be clad; Step 4: Perform laser cladding on the workpiece to be clad after surface pretreatment to form a composite powder coating on the surface of the workpiece to be clad. The laser cladding of the composite powder adopts a coaxial powder feeding method for cladding deposition. The deposition of PTFE powder adopts a high-speed spray gun powder feeding method. The high-speed spray gun and the laser cladding nozzle maintain a fixed distance. After the composite powder cladding layer is cooled to a certain temperature, the high-speed spray gun sprays the PTFE powder into the composite powder cladding layer at a high speed; Step 5: Clean the welding slag and impurities on the coating surface to obtain the laser cladding workpiece.

5. The method for preparing a laser cladding wear-resistant coating on a titanium alloy surface according to claim 4, characterized in that: In step 2, NiCoCrAlYW powder, NbN powder and BaF2 powder are ball milled by planetary ball milling, the ball milling rate is 300-500 rpm, the ball milling time is 1-3h, and the ball-to-material mass ratio is 1:(2-4).

6. The method for preparing a laser cladding wear-resistant coating on a titanium alloy surface according to claim 5, characterized in that: In step 3, the drying parameters of the composite powder and the PTFE powder are both 100-200° C. for 1-2 hours.

7. The method for preparing a laser cladding wear-resistant coating on a titanium alloy surface according to claim 6, characterized in that: The surface pretreatment in step 3 is: cutting the workpiece to be clad to the required size by wire cutting, grinding the surface of the workpiece to be clad with 80-200 mesh tungsten carbide sandpaper, and then cleaning and drying.

8. The method for preparing a laser cladding wear-resistant coating on a titanium alloy surface according to claim 7, characterized in that: In step 4, the cladding process parameters for the composite powder are: laser power 1200-1500W, laser scanning speed 5-8mm / s, powder feeding speed 12-16g / min, overlap rate 30-45%, spot diameter 3-5mm, argon protection is used during the cladding process, argon flow rate is 10-16L / min, the cladding length of each laser cladding pass is 120-150mm, and a total of 20-40 passes are performed.

9. The method for preparing a laser cladding wear-resistant coating on a titanium alloy surface according to claim 8, characterized in that: The thickness of the laser cladding wear-resistant coating is 0.8-1.2mm, and no cracks were found in the DPT flaw detection on the surface of the laser cladding wear-resistant coating.

10. A titanium alloy, characterized in that: The surface of the titanium alloy comprises a wear-resistant coating prepared by the preparation method described in any one of claims 4 to 9.