Anti-corrosion duct piece bolt and preparation method thereof
By optimizing the composition and phosphating treatment of the tube sheet bolts, combined with modified silica and other processes, the problem of insufficient strength of the tube sheet bolts is solved, significantly improving its tensile strength and corrosion resistance, ensuring the stability of the tunnel structure and security.
Patent Information
- Application Number
- CN202411494088.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-24
- Publication Date
- 2024-12-06
AI Technical Summary
The existing pipe sheet bolts are insufficient in complex geological environments, making it difficult to meet the stability and durability requirements of tunnel structures.
By optimizing the composition of the tube sheet bolts, adding elements such as Pt, Pr, Nd, etc., and using phosphating treatment, combined with rolling, heat treatment and modified silica processes, it improves its strength and corrosion resistance.
It significantly improves the tensile strength and corrosion resistance of the pipe bolts, ensuring that they maintain stable performance in harsh environments for a long time, and ensuring the safety and reliability of the tunnel structure.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fastener materials, and in particular to an anti-corrosion segment bolt and a preparation method thereof. Background Art
[0002] With the growing demand for underground space development, the scale and difficulty of tunnel construction are also increasing. Traditional tunnel construction methods often fail to meet the complex geological conditions and high engineering quality standards. Segment bolts came into being under this background and became an indispensable component of modern tunnel lining structures. Early tunnel linings mainly used materials such as bricks and stones, with relatively simple connection methods and relatively poor stability and durability. With the emergence of prefabricated concrete segments, segment bolts, as an important element for connecting these segments, began to play their unique role. Segment bolts can provide strong axial tension and shear force to ensure that the segments are tightly connected to form an integrated tunnel lining structure.
[0003] In a complex geological environment, tunnels are faced with the influence of multiple factors such as stratum pressure, groundwater, and earthquakes. Therefore, the segment bolts need to have sufficient strength to ensure that they maintain stable performance for a long time in harsh environments, thereby ensuring the safety and reliability of the tunnel structure. Summary of the invention
[0004] The present invention provides an anti-corrosion segment bolt and a preparation method thereof, which solves the problem of low strength of the segment bolt in the related art.
[0005] The technical solution of the present invention is as follows: The invention provides an anti-corrosion segment bolt, which is obtained by subjecting a segment bolt body to phosphating treatment. The segment bolt body comprises the following components by weight percentage: C 0.42%-0.5%, Si 0.17%-0.37%, Mn 0.5%-0.8%, P≤0.01%, S≤0.02%, Cu 0.07%-0.2%, Ni 1.5%-2.5%, Cr 0.5%-1.2%, Mo 0.3%-0.8%, V 0.1%-0.6%, Ti 0.08%-0.16%, Pt 0.001%-0.01%, Pr 0.01%-0.025%, Nd 0.001%-0.05%, and the rest are iron and inevitable impurities.
[0006] As a further technical solution, the weight ratio of the sum of the weights of the Pr and Nd to the weight of the Pt is 3-5:1.
[0007] In the present invention, the weight and weight ratio of Pr and Nd to Pt are limited to 3-5:1, thereby further improving the strength of the segment bolts.
[0008] As a further technical solution, the mass ratio of Pr to Nd is 4:1.
[0009] In the present invention, the strength of the segment bolts is further improved by limiting the mass ratio of Pr to Nd to 4:1.
[0010] The present invention also provides a method for preparing an anti-corrosion segment bolt, comprising the following steps: S1, after preparing the materials according to the components, melting, refining and continuous casting are performed to obtain a casting billet; S2, rolling, heat treating, drawing and threading the ingot to obtain a segment bolt body; S3, pickling, alkali washing and phosphating the segment bolt body to obtain corrosion-resistant segment bolts.
[0011] As a further technical solution, in step S3, during the phosphating, a phosphating solution is used, and the phosphating solution includes the following components in parts by weight: 17 to 30 parts of phosphoric acid, 10 to 12 parts of sodium bicarbonate, 1 to 3 parts of sodium nitrite, 10 to 15 parts of zinc nitrate, 8 to 12 parts of silicon dioxide, and 200 parts of water.
[0012] As a further technical solution, the silicon dioxide is modified silicon dioxide; the modified silicon dioxide is silicon dioxide modified by polycarbonate diol.
[0013] In the present invention, silicon dioxide is modified by polycarbonate diol, thereby further improving the corrosion resistance of the segment bolts.
[0014] As a further technical solution, the preparation method of the modified silicon dioxide comprises the following steps: dissolving polycarbonate diol in acetone, adding silicon dioxide for modification, and obtaining the modified silicon dioxide through drying.
[0015] As a further technical solution, the modification temperature is 30-40°C, and the modification time is 5-7h.
[0016] As a further technical solution, the added amount of the polycarbonate diol is 3% to 5% of the mass of the silicon dioxide.
[0017] As a further technical solution, the rolling temperature is 1100~1200℃.
[0018] As a further technical solution, the heat treatment includes quenching and tempering.
[0019] As a further technical solution, the quenching temperature is 850-900°C, and the tempering temperature is 580-600°C.
[0020] As a further technical solution, the phosphating temperature is 50-60° C., and the phosphating time is 5-10 min.
[0021] The working principle and beneficial effects of the present invention are: In the present invention, the components of the segment bolts are selected and their contents are optimized so that the segment bolts have higher strength. By adding Pt, Pr and Nd and utilizing the complementary effects of the three, the strength of the segment bolts is further improved. DETAILED DESCRIPTION
[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] In the following embodiments and comparative examples: Silica, particle size: 20 nm; polycarbonate diol, weight average molecular weight 2000; Ferrosilicon alloy, silicon content is 75wt%; ferromolybdenum alloy, molybdenum content is 70wt%; ferrovanadium alloy, vanadium content is 50wt%; ferrotitanium alloy, titanium content is 80wt%; ferromanganese alloy, manganese content is 68wt%; ferrochromium alloy, chromium content is 60wt%; platinum-iron alloy, platinum content is 38wt%; copper-neodymium alloy, neodymium content is 20wt%; nickel-praseodymium alloy, nickel content is 90wt%.
[0024] Example 1 A corrosion-resistant segment bolt is obtained by phosphating a segment bolt body, wherein the segment bolt body comprises the following components by weight percentage: C 0.42%, Si 0.17%, Mn 0.5%, P ≤0.01%, S ≤0.02%, Cu 0.07%, Ni1.5%, Cr 0.5%, Mo 0.3%, V 0.1%, Ti 0.08%, Pt 0.001%, Pr 0.01%, Nd 0.001%, and the remainder is iron and unavoidable impurities; The phosphating solution includes the following components in parts by weight: 17 parts of phosphoric acid, 10 parts of sodium bicarbonate, 1 part of sodium nitrite, 10 parts of zinc nitrate, 8 parts of silicon dioxide, and 200 parts of water; The method for preparing the corrosion-resistant segment bolts comprises the following steps: S1. Mix carbon powder, ferrosilicon alloy, ferromanganese alloy, copper block, nickel powder, ferrochromium alloy, ferromolybdenum alloy, ferrovanadium alloy, ferrotitanium alloy, ferroplatinum alloy, copper-neodymium alloy and nickel-praseodymium alloy according to the ingredients, and then melt, refine and continuously cast them to obtain ingots; S2, rolling the ingot at 1100° C., then quenching at 850° C., tempering at 580° C., drawing and threading the tempered steel to obtain the segment bolt body; S3. After pickling and alkali washing, the segment bolt body is placed in a phosphating solution at 50°C for phosphating for 10 minutes to obtain corrosion-resistant segment bolts.
[0025] Example 2 A corrosion-resistant segment bolt is obtained by phosphating a segment bolt body, wherein the segment bolt body comprises the following components by weight percentage: C 0.48%, Si 0.27%, Mn 0.65%, P ≤0.01%, S ≤0.02%, Cu 0.14%, Ni 2%, Cr 0.8%, Mo 0.5%, V 0.4%, Ti 0.12%, Pt 0.005%, Pr 0.005%, Nd 0.005%, and the remainder is iron and unavoidable impurities; The phosphating solution includes the following components in parts by weight: 23 parts of phosphoric acid, 11 parts of sodium bicarbonate, 2 parts of sodium nitrite, 13 parts of zinc nitrate, 10 parts of silicon dioxide, and 200 parts of water; The method for preparing the corrosion-resistant segment bolts comprises the following steps: S1. Mix carbon powder, ferrosilicon alloy, ferromanganese alloy, copper block, nickel powder, ferrochromium alloy, ferromolybdenum alloy, ferrovanadium alloy, ferrotitanium alloy, ferroplatinum alloy, copper-neodymium alloy and nickel-praseodymium alloy according to the ingredients, and then melt, refine and continuously cast them to obtain ingots; S2, rolling the ingot at 1150° C., then quenching it at 870° C., tempering it at 590° C., and drawing and threading the tempered steel to obtain the segment bolt body; S3. After pickling and alkali washing, the segment bolt body is placed in a phosphating solution at 55°C for phosphating for 7 minutes to obtain corrosion-resistant segment bolts.
[0026] Example 3 A corrosion-resistant segment bolt is obtained by phosphating a segment bolt body, wherein the segment bolt body comprises the following components by weight percentage: C 0.5%, Si 0.37%, Mn 0.8%, P ≤0.01%, S ≤0.02%, Cu 0.2%, Ni2.5%, Cr 1.2%, Mo 0.8%, V 0.6%, Ti 0.16%, Pt 0.01%, Pr 0.025%, Nd 0.05%, and the remainder is iron and unavoidable impurities; The phosphating solution includes the following components in parts by weight: 30 parts of phosphoric acid, 12 parts of sodium bicarbonate, 3 parts of sodium nitrite, 15 parts of zinc nitrate, 12 parts of silicon dioxide, and 200 parts of water; The method for preparing the corrosion-resistant segment bolts comprises the following steps: S1. Mix carbon powder, ferrosilicon alloy, ferromanganese alloy, copper block, nickel powder, ferrochromium alloy, ferromolybdenum alloy, ferrovanadium alloy, ferrotitanium alloy, ferroplatinum alloy, copper-neodymium alloy and nickel-praseodymium alloy according to the ingredients, and then melt, refine and continuously cast them to obtain ingots; S2, rolling the ingot at 1200° C., then quenching it at 900° C., tempering it at 600° C., and drawing and threading the tempered steel to obtain the segment bolt body; S3. After pickling and alkali washing, the segment bolt body is placed in a phosphating solution at 60°C for phosphating for 5 minutes to obtain corrosion-resistant segment bolts.
[0027] Example 4 The only difference between this embodiment and Embodiment 2 is that the segment bolt body includes the following components: C 0.48%, Si 0.27%, Mn 0.65%, P ≤0.01%, S ≤0.02%, Cu 0.14%, Ni 2%, Cr 0.8%, Mo 0.5%, V 0.4%, Ti 0.12%, Pt 0.005%, Pr 0.02%, Nd 0.02%, and the rest are iron and unavoidable impurities.
[0028] Example 5 The only difference between this embodiment and Embodiment 2 is that the segment bolt body includes the following components: C 0.48%, Si 0.27%, Mn 0.65%, P ≤0.01%, S ≤0.02%, Cu 0.14%, Ni 2%, Cr 0.8%, Mo 0.5%, V 0.4%, Ti 0.12%, Pt 0.005%, Pr 0.0075%, Nd 0.0075%, and the rest are iron and unavoidable impurities.
[0029] Example 6 The only difference between this embodiment and Embodiment 2 is that the segment bolt body includes the following components: C 0.48%, Si 0.27%, Mn 0.65%, P ≤0.01%, S ≤0.02%, Cu 0.14%, Ni 2%, Cr 0.8%, Mo 0.5%, V 0.4%, Ti 0.12%, Pt 0.005%, Pr 0.0125%, Nd 0.0125%, and the rest are iron and unavoidable impurities.
[0030] Example 7 The only difference between this embodiment and Embodiment 6 is that the segment bolt body includes the following components: C 0.48%, Si 0.27%, Mn 0.65%, P ≤0.01%, S ≤0.02%, Cu 0.14%, Ni 2%, Cr 0.8%, Mo 0.5%, V 0.4%, Ti 0.12%, Pt 0.005%, Pr 0.022%, Nd 0.003%, and the rest are iron and unavoidable impurities.
[0031] Example 8 The only difference between this embodiment and Embodiment 6 is that the segment bolt body includes the following components: C 0.48%, Si 0.27%, Mn 0.65%, P ≤0.01%, S ≤0.02%, Cu 0.14%, Ni 2%, Cr 0.8%, Mo 0.5%, V 0.4%, Ti 0.12%, Pt 0.005%, Pr 0.02%, Nd 0.005%, and the rest are iron and unavoidable impurities.
[0032] Example 9 The only difference between this embodiment and Embodiment 8 is that silicon dioxide is replaced by an equal amount of modified silicon dioxide. The preparation method of modified silicon dioxide comprises the following steps: dissolving 1.2 g of polycarbonate diol in 300 mL of acetone, adding 40 g of silicon dioxide and dispersing it evenly, heating the mixed solution to 30° C., keeping it warm and stirring for 7 hours, and obtaining modified silicon dioxide after drying.
[0033] Example 10 The only difference between this embodiment and embodiment 9 is that the preparation method of modified silica includes the following steps: dissolving 2 g of polycarbonate diol in 300 mL of acetone, adding 40 g of silica and dispersing it evenly, heating the mixed solution to 40° C., stirring at this temperature for 5 h, and obtaining modified silica after drying.
[0034] Comparative Example 1 The only difference between this comparative example and Example 1 is that the segment bolt body includes the following components: C 0.42%, Si 0.17%, Mn 0.5%, P ≤0.01%, S ≤0.02%, Cu 0.07%, Ni 1.5%, Cr 0.5%, Mo 0.3%, V 0.1%, Ti 0.08%, Pt 0.001%, Nd 0.011%, and the rest are iron and unavoidable impurities.
[0035] Comparative Example 2 The only difference between this comparative example and Example 1 is that the segment bolt body includes the following components: C 0.42%, Si 0.17%, Mn 0.5%, P ≤0.01%, S ≤0.02%, Cu 0.07%, Ni 1.5%, Cr 0.5%, Mo 0.3%, V 0.1%, Ti 0.08%, Pt 0.001%, Pr 0.011%, and the rest are iron and unavoidable impurities.
[0036] Comparative Example 3 The only difference between this comparative example and Example 1 is that the segment bolt body includes the following components: C 0.42%, Si 0.17%, Mn 0.5%, P ≤0.01%, S ≤0.02%, Cu 0.07%, Ni 1.5%, Cr 0.5%, Mo 0.3%, V 0.1%, Ti 0.08%, Pr 0.01%, Nd 0.001%, and the rest are iron and unavoidable impurities.
[0037] Comparative Example 4 The only difference between this comparative example and Example 1 is that the segment bolt body includes the following components: C 0.42%, Si 0.17%, Mn 0.5%, P ≤0.01%, S ≤0.02%, Cu 0.07%, Ni 1.5%, Cr 0.5%, Mo 0.3%, V 0.1%, Ti 0.08%, Pt 0.001%, and the rest are iron and unavoidable impurities.
[0038] Comparative Example 5 The only difference between this comparative example and Example 1 is that the segment bolt body includes the following components: C 0.42%, Si 0.17%, Mn 0.5%, P ≤0.01%, S ≤0.02%, Cu 0.07%, Ni 1.5%, Cr 0.5%, Mo 0.3%, V 0.1%, Ti0.08%, and the rest are iron and unavoidable impurities.
[0039] The tensile strength of the segment bolts prepared in Examples 1 to 8 and Comparative Examples 1 to 5 was measured according to the test method in GB / T 228.1-2021 "Tensile Test of Metallic Materials Part 1: Room Temperature Test Method"; the test results are shown in Table 1.
[0040] Table 1 Segment bolt strength performance test results
[0041] Compared with Example 1, the tensile strength of the segment bolts prepared in Comparative Examples 1 to 5 is lower than that in Example 1, indicating that when Pt, Pr, and Nd are added to the segment bolt body at the same time, the strength of the segment bolt can be improved.
[0042] Compared with Example 2, the amount of Nd added was changed in Examples 4 to 6. As a result, the tensile strength of the segment bolts prepared in Examples 5 to 6 was higher than that in Example 2, indicating that when the weight ratio of Pr and Nd to Pt is 3 to 5:1, the strength of the segment bolts can be further improved.
[0043] Compared with Example 6, the mass ratio of Pr and Nd was changed in Examples 7~8. As a result, the tensile strength of the segment bolts prepared in Example 8 was higher than those in Examples 6 and 7, indicating that when the weight ratio of the sum of Pr and Nd to Pt is 5:1 and the mass ratio of Pr and Nd is 4:1, the strength of the segment bolts can be further improved.
[0044] The corrosion resistance test of the segment bolts prepared in Example 2 and Examples 9-10 was carried out: the segment bolts were immersed in a 15wt% HCl aqueous solution for 30 minutes, and the weight loss rate of the segment bolts was tested; weight loss rate = (weight of the segment bolts before immersion - weight of the segment bolts after immersion) / weight of the segment bolts before immersion × 100%; the test results are shown in Table 2.
[0045] Table 2 Corrosion resistance test results of segment bolts
[0046] Compared with Example 2, silica was modified in Examples 9-10. As a result, the weight loss rate of the segment bolts prepared in Examples 9-10 was lower than that in Example 2, indicating that the use of polycarbonate diol to modify silica can further improve the corrosion resistance of the segment bolts.
[0047] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. An anti-corrosion segment bolt, obtained by phosphating the segment bolt body, characterized in that: Measured in percentage by weight, the segment bolt body comprises the following components: C 0.42%~0.5%, Si 0.17%~0.37%, Mn 0.5%~0.8%, P≤0.01%, S≤0.02%, Cu 0.07%~0.2%, Ni 1.5%~2.5%, Cr 0.5%~1.2%, Mo 0.3%~0.8%, V 0.1%~0.6%, Ti 0.08%~0.16%, Pt 0.001%~0.01%, Pr 0.01%~0.025%, Nd 0.001%~0.05%, and the rest are iron and unavoidable impurities.
2. The anti-corrosion segment bolt according to claim 1, characterized in that: The weight ratio of the sum of the weights of the Pr and Nd to the weight of the Pt is 3-5:
1.
3. The anti-corrosion segment bolt according to claim 2, characterized in that: The mass ratio of Pr to Nd is 4:
1.
4. The method for preparing an anti-corrosion segment bolt according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1, after preparing the materials according to the components, melting, refining and continuous casting are performed to obtain a casting billet; S2, rolling, heat treating, drawing and threading the ingot to obtain a segment bolt body; S3, pickling, alkali washing and phosphating the segment bolt body to obtain corrosion-resistant segment bolts.
5. The method for preparing anti-corrosion segment bolts according to claim 4, characterized in that: In step S3, during the phosphating, a phosphating solution is used, and the phosphating solution includes the following components in parts by weight: 17-30 parts of phosphoric acid, 10-12 parts of sodium bicarbonate, 1-3 parts of sodium nitrite, 10-15 parts of zinc nitrate, 8-12 parts of silicon dioxide, and 200 parts of water.
6. The method for preparing anti-corrosion segment bolts according to claim 5, characterized in that: The silicon dioxide is modified silicon dioxide; the modified silicon dioxide is silicon dioxide modified by polycarbonate diol.
7. The method for preparing anti-corrosion segment bolts according to claim 6, characterized in that: The added amount of the polycarbonate diol is 3% to 5% of the mass of the silicon dioxide.
8. The method for preparing anti-corrosion segment bolts according to claim 4, characterized in that: The heat treatment includes quenching and tempering.
9. The method for preparing anti-corrosion segment bolts according to claim 8, characterized in that: The quenching temperature is 850-900° C. for 3-5 hours, and the tempering temperature is 580-600° C. for 4-6 hours.
10. The method for preparing anti-corrosion segment bolts according to claim 4, characterized in that: The phosphating temperature is 50-60° C., and the phosphating time is 5-10 min.
Citation Information
Cited By
High-strength bolt and preparation method thereof
CN119710467A
High-strength bolt and preparation process thereof
CN120006167A