Method for eliminating PLC effect of heat-treatable reinforced aluminum alloy and product preparation method
By controlling the pretension rate and interval time, the PLC effect problem of aluminum alloy sheets between solid solution treatment and pretension is solved, and the uniform dislocation distribution and surface quality of aluminum alloy parts are achieved, which improves production efficiency and Performance consistency.
Patent Information
- Application Number
- CN202411201875.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
The long time interval between aluminum alloy solution treatment and pre-stretching leads to an increase in the yield strength of the sheet, which increases the difficulty of pre-stretching treatment, and reduces the production efficiency and performance consistency, leading to the emergence of the PLC effect. Impacts the surface quality and forming ability of the board.
By controlling the pre-stretching rate of the aluminum alloy between 5.0×10-5~5.0×10-4s-1, the aluminum alloy is pre-stretched, and the interval between quenching cooling and pre-stretching is no more than 12 hours , avoid the occurrence of PLC effect.
The dislocation formation speed and distribution density are reduced, and it is evenly distributed, which avoids the occurrence of PLC defects, improves production efficiency, and avoids performance degradation caused by long-term natural aging. The surface quality of the obtained aluminum alloy is qualified.
Smart Images

Figure CN119082629A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of aluminum alloy production, and in particular relates to a method for eliminating the PLC effect of heat-treatable strengthened aluminum alloy and a product preparation method. Background Art
[0002] After the solution treatment, the heat-treatable strengthened aluminum alloy plate is subjected to a pre-stretching treatment to cause permanent plastic deformation in the rolling direction of the plate and eliminate residual stress.
[0003] However, the sheet is prone to surface slip line defects (Portevin-Le Chatelier effect, referred to as PLC defects) during the pre-stretching process, which affects the surface quality defects of the sheet, causes obvious differences in the organization of different areas of the sheet, aggravates the uneven deformation of the sheet, reduces the forming ability, and even causes fracture failure.
[0004] In actual production, the PLC defect is usually avoided by extending the interval between solution treatment and stretching. After solution treatment, the plate is left to stand at room temperature, the concentration of dissolved atoms in the alloy decreases, and GP zones are continuously formed. The average movement rate of movable dislocations is reduced, making them more easily pinned by solute atoms. During this period, more atoms are concentrated toward dislocations during the waiting time, resulting in an increase in pinning strength.
[0005] The repeated pinning and depinning is the fundamental reason for the formation of PLC. Prolonging the interval between solution and stretching will increase the pinning strength of the plate, and also make it more difficult for mobile dislocations to get rid of the pinning of solid solution atoms. The plastic strain must be increased to enhance the back stress acting on the mobile dislocation. The macroscopic manifestation is that the critical tensile deformation for the occurrence of the PLC effect is increased. When the critical deformation exceeds the permanent tensile deformation required by the pre-stretching technology, the plate will not produce PLC defects.
[0006] However, extending the time interval between solution treatment and pre-stretching also reduces the residual stress elimination effect of the plate. At the same time, extending the time interval will lead to an enhanced natural aging precipitation effect, reducing the performance consistency of the plate and the plate's stress corrosion resistance.
[0007] The existing time interval can be as short as more than ten hours and as long as 2-3 days, which reduces the production efficiency of the plate, increases the difficulty of on-site production scheduling, and also increases the requirements for equipment capabilities.
[0008] In summary, the prior art obviously has inconveniences and defects in practical use, so it is necessary to improve it. Summary of the invention
[0009] In view of the above-mentioned defects, the present invention mainly provides a method for eliminating the PLC effect of heat-treatable strengthened aluminum alloys, thereby solving the technical problem that the yield strength of the plate increases due to the long time interval between the solid solution treatment and pre-stretching of the aluminum alloy, thereby increasing the difficulty of the pre-stretching treatment.
[0010] In order to solve the above problems, the present invention provides a method for eliminating the PLC effect of heat-treatable strengthened aluminum alloy, comprising the following steps:
[0011] S1, the aluminum alloy parts are solution treated and kept warm for a predetermined period of time:
[0012] S2, the aluminum alloy parts are quenched and cooled;
[0013] S3, after quenching and cooling, the aluminum alloy part is pre-stretched;
[0014] Control the pre-stretching rate not to exceed 5.0×10 -4 s -1 .
[0015] According to the method for eliminating the PLC effect of heat-treatable strengthened aluminum alloy of the present invention, the pre-stretching rate is: 5.0×10 -5 ~5.0×10 -4 s -1 .
[0016] According to the method for eliminating the PLC effect of heat-treatable strengthened aluminum alloy of the present invention, the pre-stretching rate is: 1.0×10 -4 ~5.0×10 -4 s -1 .
[0017] According to the method for eliminating the PLC effect of heat-treatable strengthened aluminum alloy of the present invention, the interval between the quenching cooling and the pre-stretching treatment does not exceed 12 hours.
[0018] According to the method for eliminating the PLC effect of heat-treatable strengthened aluminum alloy of the present invention, the interval time between the quenching cooling and the pre-stretching treatment does not exceed 30 minutes.
[0019] A product preparation method comprises the following steps:
[0020] Z1, casting heat-treatable strengthened aluminum alloy ingot;
[0021] Z2, performing homogenization heat treatment on the aluminum alloy ingot;
[0022] Z3, hot working the aluminum alloy ingot to obtain an aluminum alloy part;
[0023] Z4, using the method for eliminating the PLC effect of heat-treatable strengthened aluminum alloy to treat the aluminum alloy part.
[0024] According to the product preparation method of the present invention, the aluminum alloy ingot is subjected to homogenization heat treatment using a three-stage homogenization system, including:
[0025] Heat to 400-405°C at a heating rate of ≥40°C / h and keep warm for 3h;
[0026] Heat to 445-460℃ at a heating rate of ≥40℃ / h and keep warm for 10-24h;
[0027] Heat to 485-496°C at a heating rate of ≥30°C / h and keep warm for 8-24h.
[0028] According to the product preparation method of the present invention, the aluminum alloy ingot is thermally processed by rolling or extrusion.
[0029] According to the product preparation method of the present invention, the material of the heat-treatable and strengthened aluminum alloy part is: 2xxx, 6xxx or 7xxx series aluminum alloy.
[0030] According to the product preparation method of the present invention, the composition of the heat-treatable and strengthened aluminum alloy part is:
[0031] Si: 0~0.40%, Fe: 0~0.80%, Cu: 2.0~2.6%, Mn: 0~0.30%, Mg: 1.2~2.9%, Cr: 0~0.50%, Zn: 5.1~8.3%, Ti: 0~0.15%; the remaining components are Al.
[0032] In summary, the method for eliminating the PLC effect of heat-treatable strengthened aluminum alloys of the present invention performs pre-stretching treatment on aluminum alloy parts at a relatively low speed, thereby reducing the formation speed and distribution density of dislocations and making them uniformly distributed. During the stretching process, large-scale atomic pinning-depinning effect is difficult to occur. Therefore, PLC defects cannot be generated on the surface of the aluminum alloy parts. The present invention avoids the occurrence of the PLC effect by controlling the stretching rate. Therefore, after quenching and cooling, the aluminum alloy parts can enter the pre-stretching process without long-term natural aging, thereby improving production efficiency and avoiding performance degradation caused by long-term natural aging. The present invention also provides a product preparation method, which uses the method for eliminating the PLC effect of heat-treatable strengthened aluminum alloys to treat aluminum alloy parts to obtain products with qualified surface quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 is a surface morphology diagram of Comparative Example 1 of the present invention;
[0034] Figure 2 is a surface morphology diagram of Comparative Example 2 of the present invention;
[0035] Figure 3 is a surface topography diagram of Example 1 of the present invention;
[0036] Figure 4 is a surface topography diagram of Example 1 of the present invention;
[0037] Figure 5 is a tissue morphology diagram of Comparative Example 1 of the present invention;
[0038] Figure 6 is a tissue morphology diagram of Example 1 of the present invention;
[0039] Figure 7 is a tissue morphology diagram of Example 2 of the present invention;
[0040] in:
[0041] Figure 1-4 The surface morphology of the surface is obtained by topological morphology analyzer.
[0042] Figure 5-7 The organizational morphology was obtained by transmission electron microscopy (TEM). DETAILED DESCRIPTION
[0043] See also Figure 1 The present invention provides a method for eliminating the PLC effect of heat-treatable strengthened aluminum alloy, comprising the following steps:
[0044] S1, the aluminum alloy parts are solution treated and kept warm for a predetermined period of time:
[0045] S2, the aluminum alloy parts are quenched and cooled;
[0046] S3, after quenching and cooling, the aluminum alloy part is pre-stretched;
[0047] Control the stretching rate to: 5.0×10 -5 ~5.0×10 -4 s -1 ;
[0048] The present invention controls the stretching rate to perform pre-stretching treatment on the aluminum alloy part at a slower speed.
[0049] At a slower stretching rate, the dislocation formation rate of the aluminum alloy part is lower and the dislocation generation is more random. The gas clusters formed by the solute atoms have enough time to gather toward the mobile dislocation, so that the mobile dislocation is always in a pinned state and cannot be depinned, and it is difficult to repeatedly produce the pinning-depinning effect during the stretching process, so that the surface of the aluminum alloy part does not have PLC defects.
[0050] Combination Figure 6 and Figure 7From the perspective of dislocation distribution: under the action of the tensile rate in the above range, the dislocation distribution of the aluminum alloy parts is uniform, and the dislocation density is low. It is difficult for large-scale atomic pinning and depinning effects to occur during the stretching process. Therefore, it is difficult to produce PLC defects on the surface of the aluminum alloy parts on a macro scale.
[0051] In other words, if you want to produce PLC defects on the surface of aluminum alloy parts, you need to increase the deformation, thus increasing the critical deformation for producing PLC defects. By selecting an appropriate stretching rate so that the critical deformation is greater than the deformation specified by the pre-stretching process (such as the pre-stretching deformation required for aviation plates is: 1.5-3.0%), PLC defects can be eliminated.
[0052] The present invention performs pre-stretching treatment on the aluminum alloy parts at a slower speed, thereby reducing the formation speed and distribution density of dislocations and making them uniformly distributed. During the stretching process, large-scale atomic pinning-depinning effect is difficult to occur. Therefore, PLC defects cannot be generated on the surface of the aluminum alloy parts. The present invention avoids the occurrence of PLC defects by controlling the stretching rate. Therefore, after quenching and cooling, the aluminum alloy parts can enter the pre-stretching process without long-term natural aging, which improves production efficiency and avoids performance degradation caused by long-term natural aging.
[0053] The interval between the quenching and pre-stretching of the aluminum alloy part of the present invention is not limited, and those skilled in the art can make adaptive settings according to actual production conditions.
[0054] As an embodiment, the interval between the quenching cooling and the pre-stretching treatment of the present invention does not exceed 12 hours.
[0055] Preferably, the interval time of the present invention does not exceed 30 minutes, such as 10 minutes, 15 minutes, 20 minutes or 25 minutes, etc. After the pre-stretching treatment, the residual stress can be significantly reduced.
[0056] The present invention also provides a method for preparing the product, comprising the following steps:
[0057] Z1, casting heat-treatable strengthened aluminum alloy ingot;
[0058] Z2, performing homogenization heat treatment on the aluminum alloy ingot to eliminate residual stress and reduce chemical composition unevenness;
[0059] Preferably, the aluminum alloy ingot of the present invention is subjected to homogenization heat treatment using a three-stage homogenization system, comprising:
[0060] Heat to 400-405°C at a heating rate of ≥40°C / h and keep warm for 3h;
[0061] Heat to 445-460℃ at a heating rate of ≥40℃ / h and keep warm for 10-24h;
[0062] Heat to 485-496°C at a heating rate of ≥30°C / h and keep warm for 8-24h.
[0063] Z3, hot working the aluminum alloy ingot to obtain an aluminum alloy part;
[0064] As an embodiment, the hot working of the present invention is rolling, comprising: heating the aluminum alloy ingot to 420° C., taking it out of the furnace and rolling it into a plate;
[0065] Optionally, the rolling process of the present invention is: multiple-pass reciprocating rolling.
[0066] As an embodiment, the hot working of the present invention is extrusion, and the aluminum alloy ingot is extruded into a profile product.
[0067] Z4, treating the aluminum alloy part by using the method for eliminating the PLC effect of heat-treatable strengthened aluminum alloy;
[0068] Z5, ultrasonic nondestructive testing of aluminum alloy parts;
[0069] Z6, inspect the aluminum alloy parts and package and ship the qualified aluminum alloy parts;
[0070] The material of the heat-treatable and strengthened aluminum alloy part of the present invention is: 2xxx, 6xxx or 7xxx series aluminum alloy.
[0071] In order to verify the technical effect of the present invention, the inventors conducted a large number of experiments, and the specific experimental methods are as follows:
[0072] The present invention uses a heat-treatable and strengthened aluminum alloy, the composition of which is:
[0073] Si: 0-0.40%, Fe: 0-0.80%, Cu: 2.0-2.6%, Mn: 0-0.30%, Mg: 1.2-2.9%, Cr: 0-0.50%, Zn: 5.1-8.3%, Ti: 0-0.15%; the remaining components are Al;
[0074] The rolled plate is prepared by the product preparation method. A plurality of samples are taken from the rolled plate, and the steps of the aforementioned method for eliminating the PLC effect of heat-treatable aluminum alloy are adopted to change the stretching rate and process the sampled plates respectively. After the sample processing, the following tests are performed:
[0075] The surface morphology of the sample plate is detected by using a topological morphology analyzer;
[0076] The tissue morphology of the sample plate was detected using a transmission electron microscope (TEM);
[0077] The sample plates are respectively recorded as the embodiment and the comparative example. The differences in the processing steps and key parameters are listed below, and the similarities are not repeated here.
[0078] Embodiment 1:
[0079] The interval between the quenching cooling and pre-stretching treatment of the plate specimen is 20 min;
[0080] Control the stretching rate to: 1.0×10 -4 s -1 ; The permanent deformation of the pre-stretching treatment is 4.0%.
[0081] Embodiment 2:
[0082] The interval between the quenching cooling and pre-stretching treatment of the plate specimen is 20 min;
[0083] Control the stretching rate to: 5.0×10 -4 s -1 ; The permanent deformation of the pre-stretching treatment is 4.0%.
[0084] Comparative Example 1:
[0085] The interval between the quenching cooling and pre-stretching treatment of the plate specimen is 20 min;
[0086] Control the stretching rate to: 1.0×10 -3 s -1 ; The permanent deformation of the pre-stretching treatment is 2.0%.
[0087] Comparative Example 2:
[0088] The interval between the quenching cooling and pre-stretching treatment of the plate specimen is 20 min;
[0089] Control the stretching rate to: 6.0×10 -4 s -1 ; The permanent deformation of the pre-stretching treatment is 3.0%.
[0090] See also Figure 1-4 The samples of the two embodiments showed no PLC defects on the surface, while the samples of the two comparative examples showed obvious gully-shaped PLC defects. Moreover, the permanent deformation of the samples of the embodiments was greater than that of the samples of the comparative examples, indicating that the critical limit deformation for the occurrence of the PLC effect can be effectively increased by reducing the tensile rate.
[0091] See also Figure 5Compared with the existing stretching process parameters, the stretching rate of comparative example 1 has been reduced, and the overall number of dislocations in the sample is not large, but the dislocations are distributed in strips. During the stretching process, the matrix of the strip-shaped dislocation wall moves, which will cause the PLC effect to appear macroscopically.
[0092] See also Figure 6 and Figure 7 When the tensile rate is low enough, the dislocations in the sample are evenly distributed and the dislocation density is low. It is difficult for large-scale atomic pinning and depinning effects to occur during the tensile process. Therefore, it is difficult to generate PLC defects on the surface of aluminum alloy parts on a macro scale.
[0093] According to the results of multiple experiments, and considering the feasibility of the process parameters, in order to avoid the PLC effect, the stretching rate of the pre-stretching treatment of the present invention does not exceed 5.0×10 -4 s -1 ; For example, it can be: 1.0×10 -4 ~5.0×10 -4 s -1 ;
[0094] Based on the consideration of production cycle, production efficiency, equipment cost and product quality, the stretching rate of the pre-stretching treatment of the present invention is not less than 5.0×10 -5 s -1 ;
[0095] In order to qualitatively test the limit deformation amount at which the PLC effect occurs, the present invention further provides Example 3:
[0096] The interval between the quenching cooling and pre-stretching treatment of the plate specimen is 20 min;
[0097] Control the stretching rate to: 5.0×10 -5 s -1 ; The permanent deformation of the pre-stretching treatment is 8.0%.
[0098] No PLC effect appears on the surface of the stretched sheet, indicating that the critical limit deformation of the aluminum alloy sheet treated by the PLC effect elimination method of the present invention for the occurrence of the PLC effect exceeds 8.0%, and can meet the requirements of the pre-stretching specification with a large deformation amount.
[0099] In summary, the present invention provides a method for eliminating the PLC effect of heat-treatable strengthening aluminum alloys, by pre-stretching the aluminum alloy parts at a slower speed, reducing the formation speed and distribution density of dislocations, and making them evenly distributed. During the stretching process, large-scale atomic pinning-depinning effect is difficult to occur. Therefore, PLC defects cannot be generated on the surface of the aluminum alloy parts. The present invention avoids the occurrence of the PLC effect by controlling the stretching rate. Therefore, after quenching and cooling, the aluminum alloy parts can enter the pre-stretching process without long-term natural aging, which improves production efficiency and avoids performance degradation caused by long-term natural aging. The present invention also provides a product preparation method, which uses the method of eliminating the PLC effect of heat-treatable strengthening aluminum alloys to treat aluminum alloy parts to obtain products with qualified surface quality.
[0100] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, those skilled in the art may make various corresponding changes and modifications based on the present invention, but these corresponding changes and modifications should all fall within the scope of protection of the claims attached to the present invention.
Claims
1. A method for eliminating the PLC effect of heat-treatable strengthened aluminum alloy, characterized in that: The steps include: S1, the aluminum alloy parts are solution treated and kept warm for a predetermined period of time: S2, the aluminum alloy parts are quenched and cooled; S3, after quenching and cooling, the aluminum alloy parts are pre-stretched; Control the pre-stretching rate not to exceed 5.0×10 -4 s -1 .
2. The method for eliminating the PLC effect of heat-treatable strengthened aluminum alloy according to claim 1, characterized in that: The pre-stretching rate is: 5.0×10 -5 ~5.0×10 -4 s -1 .
3. The method for eliminating the PLC effect of heat-treatable strengthened aluminum alloy according to claim 2, characterized in that: The pre-stretching rate is: 1.0×10 -4 ~5.0×10 -4 s -1 .
4. The method for eliminating the PLC effect of heat-treatable strengthened aluminum alloy according to claim 1, characterized in that: The interval between the quenching and the pre-stretching treatment is no more than 12 hours.
5. The method for eliminating the PLC effect of heat-treatable strengthened aluminum alloy according to claim 1, characterized in that: The interval between the quenching and pre-stretching treatment does not exceed 30 minutes.
6. A product preparation method, characterized in that: The steps include: Z1, casting heat-treatable strengthened aluminum alloy ingot; Z2, performing homogenization heat treatment on the aluminum alloy ingot; Z3, hot working the aluminum alloy ingot to obtain an aluminum alloy part; Z4, treating the aluminum alloy part by using the method for eliminating the PLC effect of heat-treatable and strengthened aluminum alloy as described in any one of claims 1 to 5.
7. The product preparation method according to claim 6, characterized in that: The aluminum alloy ingot is subjected to homogenization heat treatment using a three-stage homogenization system, including: Heat to 400-405°C at a heating rate of ≥40°C / h and keep warm for 3h; Heat to 445-460℃ at a heating rate of ≥40℃ / h and keep warm for 10-24h; Heat to 485-496°C at a heating rate of ≥30°C / h and keep warm for 8-24h.
8. The method for preparing the product according to claim 6, characterized in that: The aluminum alloy ingot is hot-worked by rolling or extrusion.
9. The product preparation method according to claim 6, characterized in that: The material of the heat-treatable and strengthened aluminum alloy part is: 2xxx, 6xxx or 7xxx series aluminum alloy.
10. The product preparation method according to claim 9, characterized in that: The composition of the heat-treatable and strengthened aluminum alloy part is: Si: 0~0.40%, Fe: 0~0.80%, Cu: 2.0~2.6%, Mn: 0~0.30%, Mg: 1.2~2.9%, Cr: 0~0.50%, Zn: 5.1~8.3%, Ti: 0~0.15%; the remaining components are Al.