Method for preparing micron-sized two-dimensional grid on titanium alloy surface
By preparing micron-level two-dimensional grids on the surface of titanium alloy, using soda glass mask plate and photoresist technology, the problem of difficulty in determining interface slip in the existing technology is solved, and more accurate micro deformation analysis and structural safety are achieved. promote.
Patent Information
- Application Number
- CN202411181963.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-27
AI Technical Summary
Existing technologies such as transmission electron microscopy, scanning electron microscopy and EBSD are difficult to determine whether there is interface slippage in titanium alloy under high pressure conditions, which affects the safety and reliability of the structure.
Prepare micrometer-scale two-dimensional mesh on the surface of titanium alloy, and create clear mesh patterns using soda glass mask plate, AZ positive photoresist and gold plating technology to observe and analyze interface slip during creep.
It provides a new perspective for judging interface slip, improves the accuracy and accuracy of micro deformation mechanism analysis, and enhances the safety and reliability of the structure.
Smart Images

Figure CN119082683A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of research on microscopic deformation mechanism of materials, and in particular to a method for preparing a micron-level two-dimensional grid on the surface of a titanium alloy. Background Art
[0002] At present, titanium alloys have been used in pressure cabins and high-pressure vessels. These applications expose titanium alloys to long-term, high-load use environments. Titanium alloy pressure-resistant structures serve for a long time under high-pressure conditions, and local high-stress areas will produce creep. The cumulative plastic strain generated by creep will seriously reduce the safety and reliability of the structure. Therefore, researchers have conducted a lot of research on the low-temperature creep behavior and deformation mechanism of titanium alloys. Most of them use transmission electron microscopy, scanning electron microscopy, and EBSD to analyze the deformation mechanism of room-temperature creep of titanium alloys, such as dislocation slip, twinning, and grain boundary morphology. However, interface slip is also an important microscopic deformation mechanism. The current transmission electron microscopy, scanning electron microscopy, and EBSD cannot determine whether there is interface slip. Summary of the invention
[0003] In view of this, the present invention aims to propose a method for preparing a micrometer-level two-dimensional grid on the surface of a titanium alloy, so as to solve the problem that in the prior art, transmission electron microscopy, scanning electron microscopy and EBSD can observe deformations such as dislocations and twins, but cannot determine whether there is interface slip.
[0004] To achieve the above object, the technical solution of the present invention is achieved as follows:
[0005] A method for preparing a micrometer-scale two-dimensional grid on a titanium alloy surface comprises the following steps:
[0006] S1. Select a titanium alloy sample of a certain size and pretreat the surface of the titanium alloy sample;
[0007] S2. Prepare a continuous square grid with a line width of 1-3 μm and a line length of 10-15 μm on a soda glass mask of a certain size;
[0008] S3, coating the sample surface treated in step S1 with an AZ positive photoresist film, and then pre-baking;
[0009] S4, placing the soda glass mask obtained in step S2 on the photoresist film obtained in step S3 and exposing it to ultraviolet light for 10-60 seconds, and then post-baking;
[0010] S5. Use AZ photoresist developer to develop the post-baked sample for 40-50 seconds, and copy the square grid on the mask onto the photoresist.
[0011] S6, placing the developed sample on a hot plate for baking, evaporating the solvent to improve the adhesion between the photoresist and the sample surface;
[0012] S7, placing the sample obtained in step S6 in a magnetron sputtering device for gold plating, with a gold plating thickness of 0.5-3 μm;
[0013] S8. Place the gold-plated sample in an acetone solution to remove the photoresist, thereby obtaining a sample having a micrometer-level two-dimensional grid on the surface.
[0014] The micrometer-scale two-dimensional grid prepared on the titanium alloy surface in the present invention can be used as a reference benchmark to determine whether interface slip occurs during creep, providing a new perspective for the analysis of microscopic deformation mechanisms.
[0015] Furthermore, in step S1, the thickness of the titanium alloy sample is 0.5 mm-1 mm.
[0016] This setting not only maintains the mechanical strength and stability of the titanium alloy sample, avoiding deformation and damage of the sample during processing, but also facilitates the photoresist coating, exposure, development, gold plating, and photoresist removal processes. The thickness cooperates with the entire preparation process to make the prepared grid lines more uniform and stable, thereby improving the measurement accuracy.
[0017] Furthermore, in step S1, the pretreatment includes sequentially performing grinding treatment and polishing treatment, wherein the grinding treatment is such that no scratches can be seen by naked eyes, and the polishing treatment is such that no scratches can be seen under a microscope.
[0018] The grinding and polishing treatments set up can improve the flatness and smoothness of the sample surface, ensure the uniformity of subsequent photoresist coating, exposure effect and adhesion of the gold plating layer, and the obtained micron-level two-dimensional network has a clear and accurate grid pattern, which can more accurately analyze the interface slip and micro-deformation research mechanism in the creep process.
[0019] Furthermore, the grinding process is to use 240#, 400#, 800#, 1200#, and 2000# sandpaper containing silicon dioxide particles to grind in sequence until no scratches are visible to the naked eye.
[0020] This setting can gradually reduce the roughness of the titanium alloy surface and improve its flatness by gradually reducing the particle size of the sandpaper. This is crucial for subsequent steps such as photolithography and gold plating, because the uneven surface will affect the quality and effect of these steps.
[0021] Furthermore, the polishing treatment is firstly polishing on a polishing machine until no scratches can be seen under a microscope, and finally corroding in an etchant for 10-30 seconds.
[0022] This setting first removes tiny flaws and scratches on the surface of the titanium alloy on a polishing machine to make the surface of the titanium alloy smoother and flatter, and then treats it in an etchant for a shorter time to further refine the surface and remove tiny burrs or uneven areas that may be produced during the polishing process, thereby further improving the surface smoothness and flatness. Polishing and etching are beneficial to subsequent steps such as lithography and gold plating. The resulting micron-level two-dimensional network has a clear and accurate grid pattern, which can more accurately analyze the interface slip and micro-deformation research mechanism during the creep process.
[0023] Furthermore, when polishing with a polishing machine, the polishing machine speed is 200-400r / min, and the polishing agent is a SiO2 suspension and a H2O2 solution in a volume ratio of 1:1.
[0024] This setting improves the flatness and smoothness of the titanium alloy surface, avoids damage to the titanium alloy surface, and provides favorable conditions for the preparation of micron-level two-dimensional networks.
[0025] Furthermore, the etching agent is a mixture of hydrofluoric acid, nitric acid and water, wherein the volume ratio of hydrofluoric acid, nitric acid and water is 1:(2-3):(16-17).
[0026] Furthermore, in step S2, the thickness of the soda glass mask is 2.1-2.5 mm.
[0027] This setting enables the pattern on the mask to be clearly and accurately transferred to the photoresist. A certain thickness can further ensure the light transmittance and flatness of the mask, thereby improving the quality and accuracy of the pattern transfer.
[0028] Further, in step S3, the thickness of the AZ positive photoresist film is 0.5-3 μm.
[0029] This setup can provide multiple advantages such as high-precision pattern transfer, improved processing speed and efficiency, enhanced compatibility and stability, and reduced costs and waste.
[0030] Furthermore, in step S3, the pre-baking temperature is 80-120° C. and the time is 10-15 minutes.
[0031] In this setting, pre-baking can not only remove solvents from photoresists, improve adhesion and sensitivity, but also reduce film stress and improve process stability and repeatability. The resulting micron-scale two-dimensional network has a clear and accurate grid pattern, which can more accurately analyze the interface slip and micro-deformation research mechanism during creep.
[0032] Furthermore, in step S4, the post-baking temperature is 80-120° C. and the time is 10-30 min.
[0033] This setting can not only complete the photochemical reaction and improve the quality of the pattern, but also promote the adhesion of the photoresist to the substrate, remove residual solvents and moisture, and improve process stability and repeatability. The resulting micron-level two-dimensional network has a clear and accurate grid pattern, which can more accurately analyze the interface slip and micro-deformation research mechanism during the creep process.
[0034] Furthermore, in step S6, the temperature of the hot plate is 100-200° C., and the baking time is 10-30 min.
[0035] This setting can not only further enhance the adhesion between the photoresist and the substrate, remove residual solvents and moisture, and improve etching resistance, but also reduce stress and improve process stability and repeatability. The resulting micron-level two-dimensional network has a clear and accurate grid pattern, which can more accurately analyze the interface slip and micro-deformation research mechanism during creep.
[0036] Furthermore, the method further comprises the following steps:
[0037] S9, observing the titanium alloy sample prepared in step S8 under a metallographic microscope, measuring the line width and line length of the grid, and taking pictures of the shape of the grid lines and their positions in the grains;
[0038] S10, placing the sample in step S9 on a creep testing machine to perform a creep test;
[0039] S11. Observe the specimen after the creep test under a metallographic microscope and compare it with the metallographic photograph before the creep test to determine whether interface slip occurs during the creep process;
[0040] S111. If the grid lines passing through the grain boundary are twisted or broken, it means that interface slip has occurred during the creep process. Otherwise, interface slip has not occurred.
[0041] This setting allows for a more accurate analysis of the interface slip and micro-deformation research mechanisms during creep.
[0042] Compared with the prior art, the method for preparing a micrometer-scale two-dimensional grid on a titanium alloy surface described in the present invention has the following advantages:
[0043] (1) The grid lines on the titanium alloy surface obtained by the method of the present invention can be used as a reference. If the grid lines passing through the grain boundary are twisted or broken, it means that interface slip has occurred during the creep process, providing a new perspective for the analysis of microscopic deformation mechanism.
[0044] (2) The present invention uses a development method to copy the square grid on the mask onto the photoresist, and then obtains the titanium alloy surface grid lines through a gold plating-stripping process, which has a clear and accurate grid pattern and can more accurately analyze the interface slip and micro deformation research mechanism during the creep process;
[0045] (3) The preparation method of the present invention is simple, feasible, and has great application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 A process roadmap for preparing a micron-sized two-dimensional grid of the present invention;
[0047] Figure 2 This is a metallographic diagram of the titanium alloy sample of the present invention after polishing and corrosion;
[0048] Figure 3 This is a metallographic image of a titanium alloy surface with a gold wire grid prepared in Example 2 of the present invention. DETAILED DESCRIPTION
[0049] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0050] A method for preparing a micrometer-scale two-dimensional grid on a titanium alloy surface comprises the following steps:
[0051] S1. Select a titanium alloy sample of a certain size and pretreat the surface of the titanium alloy sample;
[0052] Specifically, the thickness of the titanium alloy sample is 0.5 mm-1 mm.
[0053] Specifically, the pretreatment includes grinding treatment and polishing treatment in sequence, wherein the grinding treatment ensures that no scratches can be seen on the surface of the titanium alloy sample by naked eyes, and the polishing treatment ensures that no scratches can be seen on the surface of the titanium alloy sample under a microscope.
[0054] Specifically, the grinding process is to use 240#, 400#, 800#, 1200#, and 2000# sandpaper containing silicon dioxide particles to grind in sequence until no scratches are visible to the naked eye;
[0055] Specifically, the polishing process is firstly polishing on a polishing machine until no scratches can be seen under a microscope, and finally corroding in an etchant.
[0056] More specifically, when polishing with a polishing machine, the polishing machine has a rotation speed of 200-400 r / min, and the polishing agent is a SiO2 suspension and a H2O2 solution in a volume ratio of 1:1.
[0057] Specifically, the etching agent is a mixture of hydrofluoric acid, nitric acid and water, wherein the volume ratio of hydrofluoric acid, nitric acid and water is 1:(2-3):(16-17). Preferably, the volume ratio of hydrofluoric acid, nitric acid and water is 5:12:83.
[0058] S2. Prepare a continuous square grid with a line width of 1-3 μm and a line length of 10-15 μm on a soda glass mask of a certain size;
[0059] The micrometer-scale two-dimensional grid prepared in this setting is not only stable, but also can more accurately determine whether interface slip occurs during creep.
[0060] Specifically, in step S2, the thickness of the soda glass mask is 2.1-2.5 mm.
[0061] S3, coating the sample surface treated in step S1 with an AZ positive photoresist film, and then pre-baking;
[0062] Specifically, in step S3, the thickness of the AZ positive photoresist film is 0.5-3 μm.
[0063] Specifically, in step S3, the pre-baking temperature is 80-120° C. and the time is 10-15 minutes.
[0064] S4, placing the soda glass mask obtained in step S2 on the photoresist film obtained in step S3 and exposing it to ultraviolet light for 10-60 seconds, and then post-baking;
[0065] Specifically, in step S4, the post-baking temperature is 80-120° C. and the time is 10-30 minutes.
[0066] S5. Use AZ photoresist developer to develop the post-baked sample for 40-50 seconds, and copy the square grid on the mask onto the photoresist.
[0067] S6, placing the developed sample on a hot plate for baking, evaporating the solvent to improve the adhesion between the photoresist and the sample surface;
[0068] Specifically, in step S6, the temperature of the hot plate is 100-200° C., and the baking time is 10-30 minutes.
[0069] S7, placing the sample obtained in step S6 in a magnetron sputtering device for gold plating, with a gold plating thickness of 0.5-3 μm;
[0070] S8. Place the gold-plated sample in an acetone solution to remove the photoresist, thereby obtaining a sample having a micrometer-level two-dimensional grid on the surface.
[0071] The present invention copies the square grid on the mask onto the photoresist by developing, and then obtains the titanium alloy surface grid lines through the gold plating-stripping process. The grid lines have a clear and accurate grid pattern, and can more accurately analyze the interface slip and micro deformation research mechanism in the creep process.
[0072] S9, observing the titanium alloy sample prepared in step S8 under a metallographic microscope, measuring the line width and line length of the grid, and taking pictures of the shape of the grid lines and their positions in the grains;
[0073] S10, placing the sample in step S9 on a creep testing machine to perform a creep test;
[0074] S11. Observe the specimen after the creep test under a metallographic microscope and compare it with the metallographic photograph before the creep test to determine whether interface slip occurs during the creep process.
[0075] S111. If the grid lines passing through the grain boundary are twisted or broken, it means that interface slip has occurred during the creep process. Otherwise, interface slip has not occurred.
[0076] The titanium alloy surface grid lines obtained by the method of the present invention can be used as a reference benchmark. If the grid lines passing through the grain boundary are twisted or broken, it means that interface slip has occurred during the creep process, providing a new perspective for the analysis of microscopic deformation mechanism. The method is simple, highly operational, and has very broad application prospects.
[0077] The technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention.
[0078] Example 1
[0079] A titanium alloy sample with a thickness of 1 mm, a length of 60 mm, and a width of 10 mm was prepared. The prepared titanium alloy sample was ground with sandpaper containing silicon dioxide particles of 240#, 400#, 800#, 1200#, and 2000# in sequence until no scratches were visible to the naked eye. It was further polished on a polishing machine until no scratches were visible under a microscope. The polishing machine speed was 200 r / min. The polishing agent was a SiO2 suspension and H2O2 solution with a volume ratio of 1:1. Finally, it was etched in an etchant composed of 5 ml of hydrofluoric acid, 12 ml of nitric acid, and 83 ml of water for 20 seconds. A continuous square grid with a grid line width of 1 μm and a line length of 10 μm was prepared on a 2.3 mm thick soda glass mask. A 0.5 μm thick AZ 1518 positive photoresist was uniformly coated on the surface of the titanium alloy after metallographic etching. Then, the photoresist film on the surface of the titanium alloy sample was pre-baked at 80°C for 15 minutes to remove the solvent and increase the adhesion between the photoresist and the titanium alloy. The prepared mask with square grid is placed on top of the photoresist film and exposed to ultraviolet light for 10 seconds. The exposed photoresist is post-baked at 80°C for 30 minutes. Then AZ 351B developer is used. AZ 351B developer is obtained by diluting deionized water and AZ 351B in a volume ratio of 4:1. After 40 seconds of development, the square grid on the mask is copied to the photoresist. The developed sample is placed on a 150°C hot plate and baked for 15 minutes to evaporate the solvent and improve the adhesion between the photoresist and the sample surface. The above sample is placed in a magnetron sputtering device for gold plating with a gold plating thickness of 0.5μm. After that, the sample is placed in an acetone solution to remove the photoresist, and a sample with a micrometer-level two-dimensional grid on the surface is obtained.
[0080] The prepared grid-line sample was observed under a metallographic microscope, the line width and length of the grid were measured, and the shape of the grid line and its position in the grain were photographed for comparison after the creep test. 0.2 , a tensile creep test with a time of 200 hours; the specimens after the creep test are observed under a metallographic microscope. If the grid lines passing through the grain boundaries are twisted or broken, it means that interface slip has occurred during the creep process.
[0081] Example 2
[0082] A titanium alloy sample with a thickness of 0.5 mm, a length of 60 mm, and a width of 10 mm was prepared. The prepared titanium alloy sample was ground with sandpaper containing silicon dioxide particles of 240#, 400#, 800#, 1200#, and 2000# in sequence until no scratches were visible to the naked eye. It was further polished on a polishing machine until no scratches were visible under a microscope. The speed of the polishing machine was 300 r / min. The polishing agent was a SiO2 suspension and a H2O2 solution in a ratio of 1:1. Finally, it was etched in an etchant consisting of 5 ml of hydrofluoric acid, 12 ml of nitric acid, and 83 ml of water for 10 seconds. A continuous square grid with a grid line width of 1 μm and a line length of 15 μm was prepared on a 2.3 mm thick soda glass mask. A 2 μm thick AZ 1518 positive photoresist was uniformly coated on the surface of the titanium alloy after metallographic etching. Then, the photoresist film on the surface of the titanium alloy sample was pre-baked at 90°C for 10 minutes to remove the solvent and increase the adhesion between the photoresist and the titanium alloy. The prepared mask with square grid is placed on top of the photoresist film and exposed to ultraviolet light for 10 seconds. The exposed photoresist is post-baked at 120°C for 30 minutes. Then, AZ 351B developer is used. AZ 351B developer is obtained by diluting deionized water and AZ 351B in a volume ratio of 4:1. After 40 seconds of development, the square grid on the mask is copied to the photoresist. The developed sample is placed on a 100°C hot plate and baked for 30 minutes to evaporate the solvent and improve the adhesion between the photoresist and the sample surface. The above sample is placed in a magnetron sputtering device for gold plating with a gold plating thickness of 3μm. After that, the sample is placed in an acetone solution to remove the photoresist, and a sample with a micrometer-level two-dimensional grid on the surface is obtained.
[0083] The prepared grid-line sample was observed under a metallographic microscope, the line width and length of the grid were measured, and the shape of the grid line and its position in the grain were photographed for comparison after the creep test. 0.2 , a tensile creep test with a time of 200 hours; the specimens after the creep test are observed under a metallographic microscope. If the grid lines passing through the grain boundaries are twisted or broken, it means that interface slip has occurred during the creep process.
[0084] Example 3
[0085] A titanium alloy sample with a thickness of 0.8 mm, a length of 60 mm, and a width of 10 mm was prepared. The prepared titanium alloy sample was ground with 240#, 400#, 800#, 1200#, and 2000# sandpaper containing silicon dioxide particles in sequence until no scratches were visible to the naked eye. It was further polished on a polishing machine until no scratches were visible under a microscope. The polishing machine speed was 400r / min, and the polishing agent was a SiO2 suspension and H2O2 solution in a ratio of 1:1. Finally, it was etched in an etchant consisting of 5ml of hydrofluoric acid, 12ml of nitric acid, and 83ml of water for 30s. A continuous square grid with a grid line width of 3μm and a line length of 10μm was prepared on a 2.3mm thick soda glass mask. A 3μm thick AZ 1518 positive photoresist was uniformly coated on the titanium alloy surface after metallographic etching, and then the photoresist film on the surface of the titanium alloy sample was pre-baked at a temperature of 120℃ for 10min to remove the solvent and increase the adhesion between the photoresist and the titanium alloy. The prepared mask with square grid is placed on top of the photoresist film and exposed to ultraviolet light for 30 seconds. The exposed photoresist is post-baked at 120°C for 30 minutes. Then AZ 351B developer is used, which is obtained by diluting deionized water and AZ 351B in a volume ratio of 4:1. After 40 seconds of development, the square grid on the mask is copied to the photoresist. The developed sample is placed on a 200°C hot plate and baked for 10 minutes to evaporate the solvent and improve the adhesion between the photoresist and the sample surface. The above sample is placed in a magnetron sputtering device for gold plating with a gold plating thickness of 1μm. After that, the sample is placed in an acetone solution to remove the photoresist, and a sample with a micrometer-level two-dimensional grid on the surface is obtained.
[0086] The prepared grid-line sample was observed under a metallographic microscope, the line width and length of the grid were measured, and the shape of the grid line and its position in the grain were photographed for comparison after the creep test. 0.2 , a tensile creep test with a time of 200 hours; the specimens after the creep test are observed under a metallographic microscope. If the grid lines passing through the grain boundaries are twisted or broken, it means that interface slip has occurred during the creep process.
[0087] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
Claims
1. A method for preparing a micrometer-scale two-dimensional grid on a titanium alloy surface, characterized in that: The steps include: S1. Select a titanium alloy sample of a certain size and pretreat the surface of the titanium alloy sample; S2. Prepare a continuous square grid with a line width of 1-3 μm and a line length of 10-15 μm on a soda glass mask of a certain size; S3, coating the sample surface treated in step S1 with an AZ positive photoresist film, and then pre-baking; S4, placing the soda glass mask obtained in step S2 on the photoresist film obtained in step S3 and exposing it to ultraviolet light for 10-60 seconds, and then post-baking; S5, using AZ photoresist supporting developer to develop the sample in step S3 for 40-50 seconds, and copy the square grid on the mask to the photoresist; S6, placing the developed sample on a hot plate for baking, evaporating the solvent to improve the adhesion between the photoresist and the sample surface; S7, placing the sample obtained in step S6 in a magnetron sputtering device for gold plating, with a gold plating thickness of 0.5-3 μm; S8. Place the gold-plated sample in an acetone solution to remove the photoresist, thereby obtaining a sample having a micrometer-level two-dimensional grid on the surface.
2. The method according to claim 1, characterized in that: In step S1, the thickness of the titanium alloy sample is 0.5 mm-1 mm.
3. The method according to claim 1, characterized in that In step S1, the pretreatment includes grinding treatment and polishing treatment in sequence, wherein the grinding treatment ensures that no scratches can be seen on the titanium alloy sample by naked eyes, and the polishing treatment ensures that no scratches can be seen on the titanium alloy sample under a microscope.
4. The method according to claim 3, characterized in that The grinding process is specifically to use 240#, 400#, 800#, 1200#, and 2000# sandpaper containing silicon dioxide particles to grind in sequence until no scratches are visible to the naked eye.
5. The method according to claim 3, characterized in that: The polishing treatment specifically includes first polishing on a polishing machine until no scratches are visible under a microscope, and finally corroding in an etchant for 10-30 seconds.
6. The method according to claim 5, characterized in that When polishing with a polishing machine, the speed of the polishing machine is 200-400r / min, and the polishing agent is a SiO2 suspension and a H2O2 solution in a volume ratio of 1:
1.
7. The method according to claim 5, characterized in that The etchant is a mixture of hydrofluoric acid, nitric acid and water, wherein the volume ratio of hydrofluoric acid, nitric acid and water is 1:(2-3):(16-17).
8. The method according to claim 1, characterized in that In step S3, the pre-baking temperature is 80-120° C. and the time is 10-15 minutes.
9. The method according to claim 1, characterized in that: In step S4, the post-baking temperature is 80-120° C. and the time is 10-30 minutes.
10. The method according to claim 1, characterized in that In step S6, the temperature of the hot plate is 100-200° C., and the baking time is 10-30 minutes.
Citation Information
Patent Citations
Metallographic corrosive, corrosion method for metallographic sample and display method for metallographic structure
CN103484863A
Manufacturing method of terahertz waveguide passive device
CN104795620A
Photoetching method of graphical sapphire substrate
CN106601601A
Mechanical polishing sampling method for cast pure titanium and titanium alloy metallographic sample
CN106908302A
Resin lens photoetched with invisible grid infrared absorption film and preparation method of resin lens
CN108415222A