Method for depositing copper on surface of PP film
By modifying 2,2'-bipyridine, modifying bipyridine additives are prepared and used in electroless copper plating solution, the problems of 2,2'-bipyridine reducing the plating rate and increasing the stress of copper film are solved, and the problem of 2,2'-bipyridine reducing the plating rate and increasing the stress of copper film is achieved. Higher plating rates and lower copper film stress improve the performance of composite fluid collections.
Patent Information
- Application Number
- CN202411203092.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Although 2,2’-bipyridine has a stable effect in the electroless copper plating process, it will reduce the plating rate and increase the stress of the copper film, affecting the performance of the composite fluid collection.
2,2'-bipyridine was modified by modifying hydroxyethylethylenediamine and sodium 4-hydroxybutylsulfonate to prepare a modified bipyridine additive and used in electroless copper plating solution to increase the plating rate and Reduce copper film stress.
The plating rate is significantly improved, while reducing the stress of the copper film and improving the performance of the composite fluid collector.
Smart Images

Figure CN119082714A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite material preparation and provides a method for copper deposition on the surface of a PP film. Background Art
[0002] Among the components of lithium batteries, the current collector is the key material for attaching active materials to the positive and negative electrodes. Traditional current collectors are pure metal foils, with aluminum foil for the positive electrode and copper foil for the negative electrode. In recent years, in order to reduce the weight of the current collector, composite current collectors have become the current development trend. Composite current collectors use polymer films as substrates, with metals plated on the upper and lower surfaces to form a sandwich-like composite structure.
[0003] "Copper-PP-copper" is a highly reliable composite current collector for the negative electrode of lithium batteries. The advantages of PP are its excellent chemical stability and corrosion resistance. The formation of a copper layer on the surface of plastic by chemical copper plating has been widely used. The basic components of chemical copper plating solution include copper salt, complexing agent, reducing agent and additives.
[0004] Commonly used copper salts include copper sulfate, copper chloride, copper nitrate, etc. Commonly used compounding agents include disodium ethylenediaminetetraacetic acid (EDTA·2Na), potassium sodium tartrate, sodium citrate, triethanolamine, etc. Commonly used reducing agents include formaldehyde, hypophosphite, hydrazine, etc. The amount of additives added is very small, but it can play a significant role. The additives for chemical copper plating mainly include stabilizers, accelerators, and surfactants.
[0005] When formaldehyde is used as a reducing agent, formaldehyde undergoes a disproportionation reaction to generate methanol and formic acid. Formic acid can 2+ Reduction to Cu + , forming Cu2O, Cu + It can also be disproportionated to generate metal Cu powder, which can act as a catalytic center to cause the decomposition of the plating solution. In the EDTA chemical copper plating system, 2,2'-bipyridine can act as a stabilizer and react with Cu + The intermediate complex Cu(Ⅰ)·(dipy)2 is formed, which is quickly oxidized by dissolved oxygen to Cu(Ⅱ)·(dipy)2, and then coordinated by EDTA with stronger coordination ability to form Cu(Ⅱ)·EDTA, thereby preventing the formation of Cu2O and Cu powder. However, the use of 2,2'-bipyridine will significantly reduce the rate of chemical copper plating. This is because 2,2'-bipyridine will adsorb on the surface of the new copper layer, hindering the formation of Cu 2+ further reduction deposition. Summary of the invention
[0006] It can be seen that although 2,2'-bipyridine has the effect of stabilizing the chemical copper plating solution, it will significantly reduce the rate of chemical copper plating. In view of this situation, the present invention proposes a method for copper deposition on the surface of PP film, which modifies 2,2'-bipyridine by hydroxyethylethylenediamine and sodium 4-hydroxybutylsulfonate, which can not only significantly increase the plating speed, but also significantly reduce the stress of the copper film.
[0007] To achieve the above purpose, the specific technical solution of the present invention is as follows:
[0008] The invention provides a method for copper deposition on the surface of a PP film, comprising the following specific steps: degreasing, roughening, neutralization, sensitization and activation, degumming, and chemical copper plating.
[0009] Preferably, the oil removal uses an aqueous solution containing 30-50 g / L sodium hydroxide, 10-30 g / L sodium carbonate, and 20-30 g / L sodium phosphate. Further preferably, the temperature of the process is 60-70°C and the time is 5-10 minutes.
[0010] Preferably, the roughening process uses an aqueous solution containing 350-400 g / L of chromium trioxide and 350-380 g / L of sulfuric acid. Further preferably, the temperature of the process is 65-75°C and the time is 10-20 min.
[0011] Preferably, the neutralization is carried out with an aqueous solution containing 50-80 g / L of sodium hydroxide. Further preferably, the temperature of the process is 20-30° C. and the time is 1-2 min.
[0012] Preferably, the sensitization and activation uses a hydrochloric acid solution containing 0.1 g / L palladium chloride and 10 g / L stannous chloride, and the concentration of hydrochloric acid is 12-13 wt %. Further preferably, the temperature of the process is 20-30° C. and the time is 25-35 min.
[0013] Preferably, the degumming process uses an aqueous solution containing 30-50 g / L of sodium hydroxide. Further preferably, the temperature of the process is 20-30° C. and the time is 2-4 min.
[0014] The invention carries out chemical copper plating on the surface of PP to prepare a "copper-PP-copper" composite material. The chemical copper plating uses copper sulfate as a copper salt, disodium ethylenediaminetetraacetate as a complexing agent, formaldehyde as a reducing agent, deionized water as a solvent, and sodium hydroxide solution to adjust the pH to 11-13.
[0015] The present invention prepares a modified bipyridine additive and uses it as an additive for chemical copper plating solution. The structural formula of the modified bipyridine additive is
[0016] The electroless copper plating solution comprises 0.04-0.06 mol / L copper sulfate, 0.06-0.08 mol / L disodium ethylenediaminetetraacetate, 10-12 ml / L formaldehyde solution (concentration 36-40 wt%), and 20-30 mg / L modified bipyridine additive.
[0017] Preferably, the electroless copper plating is performed at a temperature of 45-55° C. and for a time of 40-50 min.
[0018] The present invention provides a method for preparing the modified bipyridine additive. The preparation process of the modified bipyridine additive is as follows:
[0019] (1) Add hydroxyethylethylenediamine, di-tert-butyl dicarbonate and methanol into a reaction vessel, slowly add triethylamine dropwise under stirring, react at 10-30° C. for 6-12 hours, evaporate the solvent under reduced pressure, add water and stir, extract with ethyl acetate, dry with anhydrous sodium sulfate and filter, and evaporate under reduced pressure to obtain Boc-protected hydroxyethylethylenediamine;
[0020] (2) Add 2,2'-bipyridine-4,4'-dicarboxylic acid to thionyl chloride, heat under reflux and stir until completely dissolved, introduce nitrogen protection, add dichloromethane, Boc-protected hydroxyethylethylenediamine, and 1 / 2 triethylamine, heat under reflux for 3-5 hours, and then react at room temperature for 8-12 hours, then add sodium 4-hydroxybutylsulfonate and 1 / 2 triethylamine, heat under reflux for 4-6 hours, and then react at room temperature for 8-12 hours, wash with ultrapure water, collect the organic phase, dry with anhydrous sodium sulfate and filter, evaporate the solvent under reduced pressure, pass through a silica gel column, and then evaporate under reduced pressure and vacuum dry to obtain an intermediate product;
[0021] (3) The intermediate product is added to a saturated tetrahydrofuran solution with excess hydrogen chloride, and the reaction is stirred at room temperature for 10-12 hours to remove the Boc protection. The product is filtered, and washed with glacial ether and a dilute sodium hydroxide solution in sequence, and dried in vacuo to obtain a modified bipyridine additive.
[0022] The present invention sequentially uses hydroxyethylethylenediamine, sodium 4-hydroxybutyl sulfonate and 2,2'-bipyridine-4,4'-dicarboxylic acid to react. 2,2'-bipyridine-4,4'-dicarboxylic acid contains two reactive carboxyl groups, which can be esterified with the hydroxyl group of hydroxyethylethylenediamine to connect the amino structure with the 2,2'-bipyridine structure, or esterified with the hydroxyl group of sodium 4-hydroxybutyl sulfonate to connect the sodium sulfonate structure with the 2,2'-bipyridine structure. The above step (2) is the main process for preparing the modified bipyridine additive. Since the sulfonic acid group also has the ability to react with the hydroxyl group, the sodium sulfonate structure should be introduced later in determining the order of the two-step esterification, that is, firstly use hydroxyethylethylenediamine to react with one carboxyl group of 2,2'-bipyridine-4,4'-dicarboxylic acid, and then use sodium 4-hydroxybutyl sulfonate to react with the other carboxyl group of 2,2'-bipyridine-4,4'-dicarboxylic acid. Furthermore, the molar ratio of 2,2'-bipyridine-4,4'-dicarboxylic acid, Boc-protected hydroxyethylethylenediamine, and sodium 4-hydroxybutylsulfonate is 1:1:1. Preferably, in step (2), the amount ratio of 2,2'-bipyridine-4,4'-dicarboxylic acid, triethylamine, thionyl chloride, and dichloromethane is 1 mol: 4-5 mol: 3-5 L: 12-15 L. Further preferably, in step (2), the eluent of the silica gel column is composed of ethyl acetate and petroleum ether in a volume ratio of 1:2.
[0023] It should be noted that the structure of hydroxyethylethylenediamine contains not only hydroxyl groups but also amino groups. For the reaction with carboxyl groups, the amino groups compete with the hydroxyl groups. In order to ensure that the hydroxyl groups and carboxyl groups can smoothly undergo esterification reaction, the amino groups of hydroxyethylethylenediamine need to be protected before the reaction of step (2). Di-tert-butyl dicarbonate can remove the ester group under the action of a base (triethylamine, pyridine, etc.) to form a di-tert-butyl dicarbonate intermediate, which reacts with the amino group to protect the amino group. After the hydroxyl group reaction is completed, the protecting group can be separated from the amino group by acidic conditions. The above steps (1) and (3) are the protection process and deprotection process of the amino group, respectively. Preferably, in step (1), the amount ratio of hydroxyethylethylenediamine, di-tert-butyl dicarbonate, triethylamine, and methanol is 1 mol: 3.3-3.6 mol: 3.3-3.6 mol: 1.4-1.6 L. Further preferably, in step (1), the amount of water used is 0.8-1 times the volume of methanol; and the amount of ethyl acetate used is 3-5 times the volume of methanol.
[0024] The modified bipyridine additive used in the present invention has an amino structure introduced by hydroxyethylethylenediamine and a sodium butyl sulfonate structure introduced by sodium 4-hydroxybutyl sulfonate, in addition to a 2,2'-bipyridine structure. On the one hand, as mentioned above (see background technology), the 2,2'-bipyridine structure can reduce the generation of Cu2O and Cu powder in the plating solution, slow down the spontaneous decomposition and aging of the plating solution, and play a role in stabilizing the plating solution; on the other hand, amines have a catalytic acceleration effect on the chemical copper plating process, which can improve the Cu 2+ The deposition rate is increased to compensate for the adverse effect of 2,2'-bipyridine structure on the plating rate due to adsorption on the surface of the new copper layer. In addition, hydrogen is generated during the chemical copper plating process, and the deposited coating contains hydrogen bubbles, which will increase the stress of the deposited copper film. Sodium butyl sulfonate is a surfactant that can reduce the surface tension of the solution and promote the separation of hydrogen from the surface of the deposited copper layer, thereby reducing the effect of gas on the stress of the copper film.
[0025] Furthermore, the present invention connects the amino structure, the sodium sulfonate structure and the 2,2'-bipyridine structure together to prepare a modified bipyridine additive and add it to the chemical copper plating solution. Compared with directly adding three additives containing the amino structure, the sodium butyl sulfonate structure and the 2,2'-bipyridine structure, the method of the present invention has the following advantages: first, in the chemical copper plating process, the 2,2'-bipyridine structure has a tendency to be adsorbed on the surface of the new copper layer, so that the entire modified bipyridine additive moves toward the cathode (i.e., the PP side), driving the amino structure and the sodium butyl sulfonate structure to be unevenly distributed in the plating solution, and the closer to the PP side, the more distributed; for the amino structure, its role is to accelerate the Cu 2+ Reduction deposits on the PP surface. When it is more distributed near the PP side, it is more conducive to its role. For the sodium butyl sulfonate structure, its role is to promote the separation of hydrogen from the surface of the precipitated copper layer. Similarly, when it is more distributed near the PP side, it is more conducive to its role. Therefore, driven by the 2,2'-bipyridine structure, the acceleration effect of the amino structure and the dehydrogenation effect of the sodium butyl sulfonate structure can be significantly improved. Second, after connecting the amino structure, the sodium sulfonate structure and the 2,2'-bipyridine structure together, in the process of the 2,2'-bipyridine structure being adsorbed onto the surface of the new copper layer, the amino structure and the sodium sulfonate structure have a good affinity with the plating solution, which can reduce the adsorption tendency of the additive on the surface of the new copper layer to a certain extent, thereby reducing the adsorption of the additive to the Cu to a certain extent. 2+ Further reduction deposition is hindered, but this effect is not very obvious.
[0026] The present invention provides a method for copper deposition on the surface of a PP film. Compared with the prior art, the method has the following beneficial effects: the chemical copper plating additive of the present invention contains an amino structure, a sodium butyl sulfonate structure, and a 2,2'-bipyridine structure. The amino structure is used to increase the Cu2+ The deposition rate is increased to compensate for the adverse effect of the 2,2'-bipyridine structure on the plating rate due to adsorption on the surface of the new copper layer. The sodium butyl sulfonate structure is used to reduce the surface tension of the solution, which promotes the separation of hydrogen from the surface of the copper layer and reduces the adverse effect of the gas on the stress of the copper film. In addition, by connecting the amino structure, the sodium sulfonate structure and the 2,2'-bipyridine structure together, the acceleration effect of the amino structure and the dehydrogenation effect of the sodium sulfonate structure can be significantly improved, further increasing the plating rate and reducing the stress of the copper film. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 is the structural formula of the modified bipyridine additive of the present invention. DETAILED DESCRIPTION
[0028] The present invention is further described in detail below through specific embodiments, but this should not be construed as limiting the scope of the present invention to the following examples. Without departing from the above-mentioned method concept of the present invention, various substitutions or changes made according to common technical knowledge and conventional means in the art should be included in the scope of the present invention.
[0029] Example 1
[0030] Preparation of modified bipyridine additives:
[0031] (1) Add hydroxyethylethylenediamine, di-tert-butyl dicarbonate, and methanol into a reaction vessel, slowly add triethylamine dropwise under stirring, react at 20° C. for 9 hours, evaporate the solvent under reduced pressure, add 1 times the volume of methanol in water and stir, then extract with 4 times the volume of methanol in ethyl acetate, dry with anhydrous sodium sulfate and filter, and then evaporate under reduced pressure to obtain Boc-protected hydroxyethylethylenediamine; the amount ratio of hydroxyethylethylenediamine, di-tert-butyl dicarbonate, triethylamine, and methanol is 1 mol: 3.3 mol: 3.3 mol: 1.5 L;
[0032] (2) Add 2,2'-bipyridine-4,4'-dicarboxylic acid to thionyl chloride, heat under reflux and stir until completely dissolved, introduce nitrogen protection, add dichloromethane, Boc-protected hydroxyethylethylenediamine, and 1 / 2 triethylamine, heat under reflux for 4 h, and then react at room temperature for 10 h, then add sodium 4-hydroxybutylsulfonate and 1 / 2 triethylamine, heat under reflux for 5 h, and then react at room temperature for 10 h, wash with ultrapure water, collect the organic phase, dry with anhydrous sodium sulfate and filter, evaporate the solvent under reduced pressure, and pass through a silica gel column (the eluent is ethyl acetate). The molar ratio of 2,2'-bipyridine-4,4'-dicarboxylic acid, Boc-protected hydroxyethylethylenediamine, and sodium 4-hydroxybutylsulfonate is 1:1:1; the amount ratio of 2,2'-bipyridine-4,4'-dicarboxylic acid, Boc-protected hydroxyethylethylenediamine, sodium 4-hydroxybutylsulfonate, triethylamine, thionyl chloride, and dichloromethane is 1mol:1mol:1mol:4.5mol:4L:15L;
[0033] (3) The intermediate product was added to a saturated tetrahydrofuran solution with excess hydrogen chloride, and the reaction was stirred at room temperature for 12 h to remove the Boc protection. The product was filtered, and washed with glacial ether and a dilute sodium hydroxide solution in sequence, and dried in vacuo to obtain a modified bipyridine additive.
[0034] Copper deposition on PP film surface:
[0035] (1) Degreasing: using an aqueous solution containing 40 g / L sodium hydroxide, 20 g / L sodium carbonate, and 25 g / L sodium phosphate at 65 °C for 8 min;
[0036] (2) Roughening, using an aqueous solution containing 400 g / L chromium trioxide and 380 g / L sulfuric acid at a temperature of 70°C for 12 min;
[0037] (3) Neutralization, using an aqueous solution containing 60 g / L of sodium hydroxide at 25°C for 2 min;
[0038] (4) Sensitization and activation, using a hydrochloric acid solution containing 0.1 g / L palladium chloride and 10 g / L stannous chloride, with a hydrochloric acid concentration of 12 wt %, a temperature of 25° C., and a time of 30 min;
[0039] (5) degumming, using an aqueous solution containing 40 g / L of sodium hydroxide at 25°C for 3 min;
[0040] (6) Chemical copper plating, using an aqueous solution containing 0.05 mol / L copper sulfate, 0.07 mol / L disodium ethylenediaminetetraacetic acid, 12 ml / L formaldehyde solution (36 wt%), and 25 mg / L of the above-mentioned modified bipyridine additive, adjusting the pH to 12 with sodium hydroxide solution, the temperature is 50° C., and the time is 45 min.
[0041] Comparative Example 1
[0042] Preparation of modified bipyridine additive: Different from Example 1, 2,2'-bipyridine-4-carboxylic acid (only one carboxyl group) is used instead of 2,2'-bipyridine-4,4'-dicarboxylic acid, and only hydroxyethylethylenediamine (first protected with di-tert-butyl dicarbonate and then deprotected) is used to carry out esterification reaction with 2,2'-bipyridine-4-carboxylic acid to prepare the modified bipyridine additive. The rest is the same as Example 1.
[0043] Copper deposition on the surface of PP film: Different from Example 1, the modified bipyridine additive prepared in Comparative Example 1 is added to the chemical copper plating solution, and sodium 4-hydroxybutyl sulfonate is added, and the rest is the same as Example 1.
[0044] Comparative Example 2
[0045] Preparation of modified bipyridine additive: Same as Comparative Example 1.
[0046] Copper deposition on the surface of PP film: Different from Comparative Example 1, no sodium 4-hydroxybutane sulfonate was added to the chemical copper plating solution.
[0047] Comparative Example 3
[0048] Preparation of modified bipyridine additive: Different from Example 1, 2,2'-bipyridine-4-carboxylic acid is used instead of 2,2'-bipyridine-4,4'-dicarboxylic acid, and only sodium 4-hydroxybutyl sulfonate and 2,2'-bipyridine-4-carboxylic acid are used for esterification reaction to prepare the modified bipyridine additive. The rest is the same as Example 1.
[0049] Copper deposition on the surface of PP film: Different from Example 1, the modified bipyridine additive prepared in Comparative Example 3 is added to the chemical copper plating solution, and hydroxyethylethylenediamine is added. The rest is the same as Example 1.
[0050] Comparative Example 4
[0051] Preparation of modified bipyridine additive: Same as Comparative Example 3.
[0052] Copper deposition on the surface of PP film: Different from Comparative Example 3, hydroxyethylethylenediamine was not added to the chemical copper plating solution.
[0053] The PP film used in the above examples and comparative examples has a thickness of 4.5 μm and is purchased from Advanced Institute (Shenzhen) Technology Co., Ltd.
[0054] Performance Testing:
[0055] (1) The PP copper-plated products of Example 1, Comparative Example 3, and Comparative Example 4 were respectively used as evaluation objects, and the thickness of the copper plating layer deposited on the surface of the PP film per unit time was used as the deposition rate, and the calculation method was △m·10 4 / (ρ·A·t), △m is the mass difference before and after chemical plating (i.e., the mass of the coating, g), ρ is the copper density (g / cm 3 ), A is the coating area (cm 2 ), t is the plating time (h). The results are: the deposition rates of Example 1, Comparative Example 3, and Comparative Example 4 are 6.27μm / h, 4.52μm / h, and 2.06μm / h, respectively. It can be seen that: since Comparative Example 4 does not use hydroxyethylethylenediamine, the rate of chemical copper plating is low; Comparative Example 3 directly adds hydroxyethylethylenediamine to the plating solution, and the rate of chemical copper plating is improved; Example 1 not only uses hydroxyethylethylenediamine, but also connects it with a 2,2'-bipyridine structure, so that the rate of chemical copper plating is further improved.
[0056] (2) The PP copper-plated products of Example 1, Comparative Example 1 and Comparative Example 2 were respectively used as evaluation objects, and an X-ray diffractometer was used as a testing instrument to analyze the 2θ-sin 2 The stress of the chemical copper plating film was obtained by the ψ method; the test used a Cu-Ka target, the wavelength γ of the X-ray was 1.5406nm, the tube voltage was 40kV, the tube current was 40mA, the filter monochromator was graphite, the scanning range was 40°-100°, the scanning speed was 4° / min, and the step size was set to 0.1°. The results are as follows: the stress of the Cu(220) crystal plane of Example 1, Comparative Example 1, and Comparative Example 2 are respectively -27.55MPa ("-" indicates compressive stress), -42.71MPa, and -65.33MPa, and the stress of the Cu(311) crystal plane are respectively -41.24MPa, -57.14MPa, and -78.29MPa. It can be seen that: since sodium 4-hydroxybutyl sulfonate is not used in Comparative Example 2, the copper film stress is relatively high; in Comparative Example 1, sodium 4-hydroxybutyl sulfonate is directly added to the plating solution, the copper film stress is reduced; and in Example 1, sodium 4-hydroxybutyl sulfonate is not only used, but also connected with a 2,2'-bipyridine structure, so that the copper film stress is further reduced.
Claims
1. A method for copper deposition on the surface of a PP film, comprising the following specific steps: degreasing, roughening, neutralization, sensitization and activation, degumming, and chemical copper plating; the chemical copper plating solution is composed of 0.04-0.06 mol / L copper sulfate, 0.06-0.08 mol / L disodium ethylenediaminetetraacetic acid, 10-12 ml / L formaldehyde solution (concentration 36-40 wt%), and 20-30 mg / L additives, the solvent is deionized water, and the pH is adjusted to 11-13 with sodium hydroxide solution; Features: The additive is a modified bipyridine additive; the structural formula of the modified bipyridine additive is 2. The method for copper deposition on the surface of a PP film according to claim 1, characterized in that: The oil removal uses an aqueous solution containing 30-50g / L sodium hydroxide, 10-30g / L sodium carbonate, and 20-30g / L sodium phosphate, at a temperature of 60-70°C for 5-10min; The roughening process uses an aqueous solution containing 350-400 g / L chromium trioxide and 350-380 g / L sulfuric acid at a temperature of 65-75° C. for 10-20 min. The neutralization is carried out using an aqueous solution containing 50-80 g / L of sodium hydroxide at a temperature of 20-30° C. for 1-2 min; The sensitization and activation adopts a hydrochloric acid solution containing 0.1g / L palladium chloride and 10g / L stannous chloride, the hydrochloric acid concentration is 12-13wt%, the temperature is 20-30°C, and the time is 25-35min; The degumming process uses an aqueous solution containing 30-50 g / L of sodium hydroxide at a temperature of 20-30° C. for 2-4 minutes.
3. The method for copper deposition on the surface of a PP film according to claim 1, characterized in that: The electroless copper plating temperature is 45-55° C. and the time is 40-50 min.
4. The method for copper deposition on the surface of a PP film according to claim 1, characterized in that: The preparation process of the modified bipyridine additive is as follows: (1) Add hydroxyethylethylenediamine, di-tert-butyl dicarbonate and methanol into a reaction vessel, slowly add triethylamine dropwise under stirring, react at 10-30° C. for 6-12 hours, evaporate the solvent under reduced pressure, add water and stir, extract with ethyl acetate, dry with anhydrous sodium sulfate and filter, and evaporate under reduced pressure to obtain Boc-protected hydroxyethylethylenediamine; (2) Add 2,2'-bipyridine-4,4'-dicarboxylic acid to thionyl chloride, heat under reflux and stir until completely dissolved, introduce nitrogen protection, add dichloromethane, Boc-protected hydroxyethylethylenediamine, and 1 / 2 triethylamine, heat under reflux for 3-5 hours, and then react at room temperature for 8-12 hours, then add sodium 4-hydroxybutylsulfonate and 1 / 2 triethylamine, heat under reflux for 4-6 hours, and then react at room temperature for 8-12 hours, wash with ultrapure water, collect the organic phase, dry with anhydrous sodium sulfate and filter, evaporate the solvent under reduced pressure, pass through a silica gel column, and then evaporate under reduced pressure and vacuum dry to obtain an intermediate product; The molar ratio of 2,2'-bipyridine-4,4'-dicarboxylic acid, Boc-protected hydroxyethylethylenediamine, and sodium 4-hydroxybutylsulfonate is 1:1:1; (3) The intermediate product is added to a saturated tetrahydrofuran solution with excess hydrogen chloride, and the reaction is stirred at room temperature for 10-12 hours to remove the Boc protection. The product is filtered, and washed with glacial ether and a dilute sodium hydroxide solution in sequence, and dried in vacuo to obtain a modified bipyridine additive.
5. The method for copper deposition on the surface of a PP film according to claim 4, characterized in that: In step (1), the usage ratio of hydroxyethylethylenediamine, di-tert-butyl dicarbonate, triethylamine and methanol is 1 mol: 3.3-3.6 mol: 3.3-3.6 mol: 1.4-1.6 L.
6. The method for copper deposition on the surface of a PP film according to claim 4, characterized in that: In step (1), the amount of water used is 0.8-1 times the volume of methanol; the amount of ethyl acetate used is 3-5 times the volume of methanol.
7. The method for copper deposition on the surface of a PP film according to claim 4, characterized in that: In step (2), the usage ratio of 2,2'-bipyridine-4,4'-dicarboxylic acid, triethylamine, thionyl chloride and dichloromethane is 1 mol: 4-5 mol: 3-5 L: 12-15 L.
8. The method for copper deposition on the surface of a PP film according to claim 4, characterized in that: In step (2), the eluent of the silica gel column is composed of ethyl acetate and petroleum ether in a volume ratio of 1:2.