Inclined perforated porous transmission layer in proton exchange membrane electrolytic cell

By creating oblique perforations on the porous transport layer of the proton exchange membrane electrolytic cell, the problems of oxygen accumulation and water shortage at high current density are solved, and the performance and efficiency of the electrolytic cell are improved. It is suitable for different types of bipolar plate flow channel structures .

CN119082757APending Publication Date: 2024-12-06HARBIN INSTITUTE OF TECHNOLOGY (SHENZHEN) (INSTITUTE OF SCIENCE AND TECHNOLOGY INNOVATION HARBIN INSTITUTE OF TECHNOLOGY SHENZHEN)
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411297427.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In proton exchange membrane electrolytic cell, oxygen accumulation and local water shortage are serious under high current density, resulting in mass transfer losses and hot spots, hindering the improvement of battery performance. The existing technology has failed to effectively solve the low oxygen removal efficiency under bipolar plate ribs The problem.

Method used

By using an oblique perforated porous transport layer structure, by making oblique perforated on the porous transport layer, priority channels are provided to accelerate oxygen exhaust, reduce oxygen accumulation, and improve gas-liquid flow and material transfer efficiency.

Benefits of technology

The two-phase flow of gas and liquid inside the electrolytic cell is significantly improved, the accumulation of oxygen in the porous transport layer is reduced, water starvation and local hot spots are prevented, and the electrochemical performance of the electrolytic cell is improved under high current density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082757A_ABST
    Figure CN119082757A_ABST
Patent Text Reader

Abstract

The invention discloses an inclined perforated porous transmission layer in a proton exchange membrane electrolytic cell, and belongs to the technical field of proton exchange membrane water electrolysis. By analyzing the flow characteristics of liquid water and oxygen in the porous transmission layer of the proton exchange membrane electrolytic cell and analyzing the influence of the existence of the rib plate of the bipolar plate on the oxygen removal efficiency, the invention provides a porous transmission layer structure optimization technology, namely an inclined perforation technology, for promoting the removal of oxygen under the rib plate. The inclined perforated porous transmission layer manufactured on the basis can provide a priority channel for oxygen transportation, effectively optimizes gas-liquid two-phase flow and material transfer efficiency in the electrolytic cell, promotes supply of liquid water and elimination of generated oxygen, and accordingly improves the overall performance of the electrolytic cell. In conclusion, a brand-new porous transmission layer structure optimization scheme beneficial to improvement of the performance of the proton exchange membrane electrolytic cell can be provided for the proton exchange membrane electrolytic cell, and the proton exchange membrane electrolytic cell has very wide market prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of proton exchange membrane water electrolysis, and in particular relates to an obliquely perforated porous transmission layer in a proton exchange membrane electrolyzer. Background Art

[0002] Hydrogen is an ideal clean energy fuel and is expected to replace traditional fossil fuel energy in the future. In addition, the acquisition of hydrogen energy can also be combined with renewable energy. The entire process of its energy cycle is completely carbon-free and is a truly clean process. At present, water electrolysis hydrogen production technology is the most effective means of obtaining hydrogen energy and is considered to be a key element of the future sustainable energy system.

[0003] Proton exchange membrane electrolyzer is a kind of hydrogen production technology by electrolysis of water. Compared with other types of electrolyzers (such as alkaline electrolyzers, solid oxide electrolyzers, etc.), it has considerable performance advantages in the era of rapid development of renewable energy: such as it can operate under low temperature conditions, has extremely high energy conversion efficiency, can obtain extremely high purity hydrogen, has a wide voltage application range, extremely compact multilayer structure, and fast renewable energy response, etc. With the rapid transformation of energy structure and the rapid development of renewable energy, the industry has higher and higher requirements for the performance of future electrolyzers, especially requiring them to be able to work stably and reliably under high voltage and high current density (current density>5A / cm 2 ). However, as the current density increases, serious oxygen accumulation and water shortage will occur inside the proton exchange membrane electrolyzer, making mass transfer loss the largest contributor to the improvement of battery performance among all loss mechanisms. When the operating current density of the electrolyzer is 1A / cm 2 , material transport losses already account for 20% to 25% of the total overpotential. In addition, during this process, the transport directions of liquid water and oxygen are completely opposite, which will lead to unnecessary viscous dissipation and hinder the transport of liquid water and oxygen. More importantly, the accumulated oxygen bubbles are likely to be trapped in the porous transport layer, preventing liquid water from entering, causing local water shortages and generating hot spots, interfering with the continued chemical reaction, and ultimately seriously hindering the performance of the electrolyzer. In summary, at high current density, the mass transfer loss caused by gas-liquid transport will become more prominent, seriously hindering the development of proton exchange membrane electrolyzers towards high current operation modes, and unable to meet the long-term development goals of combining renewable energy with electrolyzers. It can be seen that gas-liquid management inside the electrolyzer is particularly important in the future development of proton exchange membrane electrolyzers.

[0004] In recent years, people have made a lot of efforts to optimize the mass transfer inside the proton exchange membrane electrolyzer, especially the gas-liquid two-phase mass transfer in the porous transport layer. For example, by changing the hydrophilicity of different areas of the porous transport layer, or adjusting the microscopic parameters of the porous transport layer such as porosity, permeability, pore size, etc., the gas-liquid flow in the porous transport layer can be optimized to a certain extent. However, no one has yet proposed a targeted and reliable solution to the severe oxygen accumulation in the porous transport layer under the bipolar plate ribs and the resulting local hot spots and local water starvation. Summary of the invention

[0005] In view of the above technical background, the present invention analyzes the flow characteristics of liquid water and oxygen in the porous transport layer of the proton exchange membrane electrolyzer, analyzes the influence of the existence of the bipolar plate ribs on the oxygen removal efficiency, and proposes a porous transport layer structure optimization technology to promote the removal of oxygen under the bipolar plate ribs - oblique perforation technology. The oblique perforated porous transport layer manufactured based on this can provide a priority channel for the transportation of oxygen, effectively optimizes the gas-liquid two-phase flow and material transfer efficiency inside the electrolyzer, promotes the supply of liquid water and the removal of generated oxygen, thereby improving the overall performance of the electrolyzer. In short, the present invention can provide a new porous transport layer structure optimization solution for proton exchange membrane electrolyzers that helps improve their performance, and has a very broad market prospect.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] One of the technical solutions of the present invention is to provide an obliquely perforated porous transport layer in a proton exchange membrane electrolyzer, wherein the two ends of the oblique perforations of the obliquely perforated porous transport layer face the bipolar plate and the catalyst layer respectively, wherein the end of the oblique perforation facing the bipolar plate is connected to the flow channel, and the end facing the catalyst layer is located directly below the bipolar plate rib.

[0008] Preferably, the manufacturing method of the oblique perforations includes mechanical perforation method, jet perforation method and laser perforation method.

[0009] More preferably, the steps of the mechanical perforation method include: cleaning the original porous transport layer and trimming its surface; determining the section of the porous transport layer in contact with the bipolar plate flow channel, and marking the position of the oblique perforation according to the oblique perforation scheme; at the oblique perforation position, according to the thickness of the porous transport layer and the flow channel-rib plate distribution, determining the diameter and angle of the oblique perforation, so that the two ends of the oblique perforation are respectively located at the flow channel section facing the bipolar plate and the rib plate section facing the catalyst layer; using a drill bit to obliquely drill holes in the porous transport layer or using a reamer to obliquely ream the porous transport layer to form holes, such as Figure 4 As shown in (a).

[0010] More preferably, the steps of the jet perforation method include: cleaning the original porous transport layer and trimming its surface; determining the section of the porous transport layer in contact with the bipolar plate flow channel, and marking the position of the oblique perforation according to the oblique perforation scheme; at the oblique perforation position, according to the thickness of the porous transport layer and the flow channel-rib plate distribution, determining the diameter and angle of the oblique perforation, so that the two ends of the oblique perforation are respectively located in the flow channel section facing the bipolar plate and the rib plate section facing the catalyst layer; using high-speed jet abrasive particles or water flow to impact the surface of the porous transport layer to form holes, such as Figure 4 As shown in (b).

[0011] More preferably, the steps of the laser perforation method include: cleaning the original porous transport layer and trimming its surface; determining the section of the porous transport layer in contact with the bipolar plate flow channel, and marking the position of the oblique perforation according to the oblique perforation scheme; at the oblique perforation position, according to the thickness of the porous transport layer and the flow channel-rib plate distribution, determining the diameter and angle of the oblique perforation, so that the two ends of the oblique perforation are respectively located in the flow channel section facing the bipolar plate and the rib plate section facing the catalyst layer; using a laser beam to irradiate the surface of the porous transport layer to form holes, such as Figure 4 As shown in (c).

[0012] Preferably, for the serpentine flow channel proton exchange membrane electrolyzer, the porous transport layer adopts an oblique perforation scheme in which oblique holes are opened from the surface of each serpentine flow channel section on one side of the bipolar plate, along the flow direction, in sequence obliquely toward the corresponding rib plate section on the catalyst layer side.

[0013] Preferably, for a parallel flow channel proton exchange membrane electrolyzer, an oblique perforation scheme is adopted for the porous transport layer: oblique holes are opened from the surface of each parallel flow channel section on one side of the bipolar plate, along the flow direction, in sequence obliquely toward the corresponding rib plate section on one side of the catalyst layer.

[0014] Preferably, for the interdigitated channel proton exchange membrane electrolyzer, the porous transport layer adopts an oblique perforation scheme in which oblique holes are opened in sequence along the flow direction from the surface of each parallel channel section connected to the outlet manifold on one side of the bipolar plate to the corresponding rib plate section on one side of the catalyst layer.

[0015] Preferably, for the serpentine-parallel mixed channel proton exchange membrane electrolyzer, the porous transport layer adopts an oblique perforation scheme in which oblique holes are opened from the surface of each serpentine channel section on one side of the bipolar plate, along the flow direction, in sequence toward the corresponding rib plate section on the catalyst layer side.

[0016] The second technical solution of the present invention: Application of the obliquely perforated porous transport layer in the above-mentioned proton exchange membrane electrolyzer in a proton exchange membrane electrolyzer.

[0017] The working principle of the oblique perforated porous transmission layer in the present invention is:

[0018] For a proton exchange membrane electrolyzer, it is usually necessary to punch or etch flow channels on its bipolar plates, through which water and oxygen are transported, thereby achieving the supply of reactants and the removal of products. Figure 1 As shown, for the classic parallel flow channel ( Figure 1 (a)), serpentine flow channel ( Figure 1 (b)), interdigital flow channel ( Figure 1 (c)) and serpentine-parallel flow channels ( Figure 1 In (d), the flow channels and ribs on the bipolar plates always appear alternately, and their forms are slightly different.

[0019] The bipolar plate is in close contact with the porous transport layer, where the contact part has both flow channel area and rib plate area, which exist alternately, such as Figure 2 As shown, (a) is a schematic diagram of the flow path of oxygen bubbles generated below the ribs in the porous transport layer, and (b) is an image of the flow pattern of oxygen bubbles generated below the ribs breaking through from their generation points into the flow channel. It can be found that since part of the area on the bipolar plate that contacts the porous transport layer is the ribs, the presence of these ribs will hinder the transport of oxygen to a certain extent, thereby causing oxygen to accumulate in the porous transport layer below the bipolar plate ribs, which will seriously damage the performance of the proton exchange membrane electrolyzer. In view of this, the present invention creatively proposes an oblique perforation technology for the porous transport layer, and the oblique perforation position is as follows: Figure 3 As shown: The oblique perforations can provide a low-resistance channel for oxygen in the porous transport layer under the ribs to enter the flow channel, thereby accelerating the discharge of oxygen in the porous transport layer, alleviating water starvation and the generation of local hot spots, and improving the electrochemical performance of the electrolyzer operating at high current density.

[0020] The beneficial technical effects of the present invention are as follows:

[0021] (1) In view of the common characteristics of alternating "channel-rib" in the bipolar plate of the proton exchange membrane electrolyzer, the "channel-rib" oblique perforation process design is adopted for the porous transport layer, which significantly improves the effect of gas-liquid two-phase flow in the porous transport layer, accelerates oxygen discharge, and reduces mass transfer loss.

[0022] (2) The “channel-rib” oblique perforation optimization strategy does not require major changes to the existing structure of the proton exchange membrane electrolyzer, nor does it require the addition of additional system accessories. It can be achieved by only performing small perforations on the porous transport layer, which is very compatible with the existing electrolyzer production process.

[0023] (3) The “channel-rib” oblique perforation optimization strategy is particularly suitable for large-scale proton exchange membrane electrolyzers. In view of the characteristics of vigorous oxygen generation and severe oxygen accumulation under high current density, the oblique perforation method can significantly reduce the accumulation of oxygen in the porous transport layer, thereby effectively preventing the occurrence of water starvation and local hot spots under high current density.

[0024] (4) The “channel-rib” oblique perforation optimization strategy can be fully applied to different types of bipolar plate channel structures. According to the staggered appearance of the “channel-rib” structure, a targeted oblique perforation design suitable for the structure can be proposed, which has a wide range of applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 Schematic diagrams of bipolar plates in a proton exchange membrane electrolyzer, wherein (a) is a schematic diagram of a bipolar plate with parallel flow channels, (b) is a schematic diagram of a bipolar plate with serpentine flow channels, (c) is a schematic diagram of a bipolar plate with interdigitated flow channels, and (d) is a schematic diagram of a bipolar plate with serpentine-parallel flow channels.

[0026] Figure 2 Schematic diagram of oxygen breaking through the porous transport layer to the flow channel in a proton exchange membrane electrolyzer, wherein (a) is a schematic diagram of the flow path of oxygen bubbles generated below the ribs in the porous transport layer, and (b) is an image of the flow pattern of oxygen bubbles generated below the ribs breaking through from their generation points into the flow channel.

[0027] Figure 3 Schematic diagram of the path of oxygen breaking through the porous transport layer to the flow channel in a proton exchange membrane electrolyzer after adopting the "flow channel-rib plate" oblique perforation scheme.

[0028] Figure 4 Schematic diagrams of different perforation methods for obliquely perforated porous transmission layers, where (a) is a schematic diagram of mechanical perforation, (b) is a schematic diagram of jet perforation, and (c) is a schematic diagram of laser perforation.

[0029] Figure 5 This is an implementation case of the oblique perforation of the porous transport layer in the serpentine flow channel proton exchange membrane electrolyzer in Example 1.

[0030] Figure 6 This is an implementation case of the oblique perforation of the porous transport layer in the parallel flow channel proton exchange membrane electrolyzer in Example 2.

[0031] Figure 7 This is an implementation case of the oblique perforation of the porous transport layer in the interdigitated flow channel proton exchange membrane electrolyzer in Example 3.

[0032] Figure 8 This is an implementation case of the oblique perforation of the porous transport layer in the serpentine-parallel mixed flow channel proton exchange membrane electrolyzer in Example 4.

[0033] Fig. 9 This is the flow pattern image of oxygen breaking through the porous transmission layer to the flow channel when the center of the oblique perforation is 100 microns away from the oxygen generation center and the perforation diameter is 110 microns.

[0034] Fig.10 This is the flow pattern image of oxygen breaking through the porous transmission layer to the flow channel when the center of the oblique perforation is 100 microns away from the oxygen generation center and the perforation diameter is 120 microns.

[0035] Fig.11 This is the flow pattern image of oxygen breaking through the porous transmission layer to the flow channel when the center of the oblique perforation is 190 microns away from the oxygen generation center and the perforation diameter is 120 microns.

[0036] Fig.12 This is the curve of the average saturation of oxygen in the porous transport layer changing with time at different oblique perforation positions and diameters.

[0037] Fig.13 This is the curve of the average escape velocity of oxygen in the porous transport layer changing with time at different oblique perforation positions and diameters. DETAILED DESCRIPTION

[0038] Now, various exemplary embodiments of the present invention are described in detail, and this detailed description should not be considered as a limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing specific embodiments and are not used to limit the present invention.

[0039] In addition, for the numerical range in the present invention, it is understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0040] Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the invention pertains. Although only preferred methods and materials are described herein, any methods and materials similar or equivalent to those described herein may also be used in the practice or testing of the present invention.

[0041] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0042] Example 1

[0043] Implementation case of porous transport layer for serpentine flow channel proton exchange membrane electrolyzer (schematic diagram see Figure 5 ):

[0044] The serpentine flow channel is formed by bending a single channel into nine parallel sections. Figure 5The blue area represents the porous transport layer surface in contact with the flow channel, and the gray area represents the porous transport layer surface in contact with the ribs. Figure 5 As shown, for the surface of the porous transport layer that contacts each section of the serpentine flow channel, six inclined holes are opened at equal intervals, and each inclined hole extends obliquely downward from the blue area to the adjacent gray area to the catalyst layer, thereby providing a low-resistance path to the flow channel for the oxygen accumulated in the porous transport layer under the ribs. Specifically, first mark the area of ​​the porous transport layer close to the flow channel, then determine the perforation position (a total of 6×9=54 holes in this case), the perforation radius and the perforation angle, and then implement the perforation process in sequence. After all the oblique through holes are processed, a porous transport layer with a special "flow channel-rib plate" oblique perforation structure can be obtained.

[0045] The above implementation only represents some of the serpentine flow channel porous transport layer oblique perforation schemes, which can be further promoted by analogy (such as adjusting the number of perforations, perforation points, perforation angles, perforation radius, etc.). The two ends of the oblique perforations of the porous transport layer are respectively located in the flow channel section (facing the bipolar plate) and the rib section (facing the catalyst layer). Its advantage is that it can provide a low-resistance flow path directly to the flow channel for the oxygen under the ribs of the serpentine flow channel bipolar plate, reduce the oxygen saturation in the porous transport layer, and thus optimize the performance of the electrolytic cell; its disadvantage is that it makes the preparation process of the porous transport layer more complicated, increases the processing difficulty and precision requirements of the electrolytic cell, and has a certain negative effect on the mechanical strength of the porous transport layer.

[0046] Example 2

[0047] Implementation case of porous transport layer for parallel flow proton exchange membrane electrolyzer (schematic diagram see Figure 6 ):

[0048] The parallel flow channel is composed of an inlet main channel, an outlet main channel and nine parallel sub-channels. Figure 6 The blue area represents the porous transport layer surface in contact with the flow channel, and the gray area represents the porous transport layer surface in contact with the ribs. Figure 6 As shown, for the surface of the porous transport layer that contacts each parallel sub-channel, six inclined holes are opened at equal intervals, and each inclined hole extends obliquely downward from the blue area to the adjacent gray area to the catalyst layer, thereby providing a low-resistance path to the flow channel for the oxygen accumulated in the porous transport layer under the ribs. Specifically, first mark the area of ​​the porous transport layer close to the flow channel, then determine the perforation position (a total of 6×9=54 holes in this case), the perforation radius and the perforation angle, and then implement the perforation process in sequence. After all the oblique through holes are processed, a porous transport layer with a special "flow channel-rib" oblique perforation structure can be obtained.

[0049] The above implementation only represents some parallel flow channel porous transport layer oblique perforation schemes, which can be further promoted by analogy (such as adjusting the number of perforations, perforation points, perforation angles, perforation radius, etc.). The two ends of the oblique perforations of the porous transport layer are respectively located in the flow channel section (facing the bipolar plate) and the rib section (facing the catalyst layer). Its advantage is that it can provide a low-resistance flow path directly to the flow channel for the oxygen under the ribs of the parallel flow channel bipolar plate, reduce the oxygen saturation in the porous transport layer, and thus optimize the performance of the electrolytic cell; its disadvantage is that it makes the preparation process of the porous transport layer more complicated, increases the processing difficulty and precision requirements of the electrolytic cell, and has a certain negative effect on the mechanical strength of the porous transport layer.

[0050] Example 3

[0051] Implementation case of porous transport layer for interdigitated channel proton exchange membrane electrolyzer (schematic diagram see Figure 7 ):

[0052] The interdigital flow channel is composed of an inlet manifold, an outlet manifold and nine parallel sub-channels, wherein the sub-channel connected to the inlet manifold is the inlet sub-channel, and the sub-channel connected to the outlet manifold is the outlet sub-channel. Figure 7 The blue area represents the porous transport layer surface in contact with the flow channel, and the gray area represents the porous transport layer surface in contact with the ribs. Figure 7 As shown, for the surface of the porous transport layer that contacts each outlet sub-channel, six inclined holes are opened at equal intervals, and each inclined hole leads from the blue area to the adjacent gray area obliquely to the left and right respectively until the catalyst layer, providing a low-resistance path to the outlet flow channel for the oxygen accumulated under the ribs of the porous transport layer. Specifically, first mark the area of ​​the porous transport layer close to the flow channel, then determine the perforation position (a total of 6×4=24 holes in this case), the perforation radius and the perforation angle, and then implement the perforation process in sequence. After all the oblique through holes are processed, a porous transport layer with a special "flow channel-rib" oblique perforation structure can be obtained.

[0053] The above implementation only represents the oblique perforation scheme of the porous transport layer of the interdigitated flow channel, and can be further promoted by analogy (such as adjusting the number of perforations, perforation points, perforation angles, perforation radius, etc.). The two ends of the oblique perforations of the porous transport layer are respectively located in the flow channel section (facing the bipolar plate) and the rib section (facing the catalyst layer). Its advantage is that it can provide a low-resistance flow path directly to the outlet flow channel for the oxygen under the ribs of the bipolar plate of the interdigitated flow channel, reduce the oxygen saturation in the porous transport layer, and thus optimize the performance of the electrolytic cell; its disadvantage is that it makes the preparation process of the porous transport layer more complicated, increases the processing difficulty and precision requirements of the electrolytic cell, and has a certain negative effect on the mechanical strength of the porous transport layer.

[0054] Example 4

[0055] Implementation case of porous transport layer for serpentine-parallel mixed flow channel proton exchange membrane electrolyzer (schematic diagram see Figure 8 ):

[0056] The serpentine-parallel mixing channel is composed of an inlet main channel, an outlet main channel and three serpentine sub-channels that are bent three times and parallel to each other. Figure 8 The blue area represents the porous transport layer surface in contact with the flow channel, and the gray area represents the porous transport layer surface in contact with the ribs. Figure 8 As shown, for the surface of the porous transport layer that contacts each serpentine sub-channel, 18 oblique holes are opened in sequence along the flow path of the serpentine sub-channel, and each oblique hole leads obliquely downward from the blue area to the adjacent gray area to the catalyst layer, thereby providing a low-resistance path to the flow channel for the oxygen accumulated under the ribs of the porous transport layer. Specifically, first mark the area of ​​the porous transport layer close to the flow channel, then determine the perforation position (a total of 18×3=54 holes in this case), the perforation radius and the perforation angle, and then implement the perforation process in sequence. After all the oblique through holes are processed, a porous transport layer with a special "flow channel-rib" oblique perforation structure can be obtained.

[0057] The above implementation only represents some of the serpentine-parallel mixing channel porous transport layer oblique perforation schemes, which can be further promoted by analogy (such as adjusting the number of perforations, perforation points, perforation angles, perforation radius, etc.). The two ends of the oblique perforations of the porous transport layer are respectively located in the flow channel section (facing the bipolar plate) and the rib section (facing the catalyst layer). Its advantage is that it can provide a flow path directly to the flow channel for the oxygen under the ribs of the serpentine-parallel mixing channel bipolar plate, reduce the oxygen saturation in the porous transport layer, and thus optimize the performance of the electrolytic cell; its disadvantage is that it makes the preparation process of the porous transport layer more complicated, increases the processing difficulty and precision requirements of the electrolytic cell, and has a certain negative effect on the mechanical strength of the porous transport layer.

[0058] Although the above implementation cases only involve four types of flow channels, namely serpentine, parallel, interdigitated and serpentine-parallel mixed, the core idea of ​​oblique perforation of the porous transport layer by "flow channel-rib plate" can be extrapolated to the porous transport layer corresponding to any flow channel structure, such as annular flow channels, spiral flow channels and point flow channels.

[0059] Performance:

[0060] The degassing performance of the oblique perforation of the porous transmission layer in the present invention mainly depends on the perforation position and the perforation radius. Now take an oblique perforation unit in the oblique perforation method of Example 1, and consider a certain oxygen generation point under the rib plate, and analyze the contribution of the oblique perforation technology of the porous transmission layer to oxygen removal for different perforation positions and perforation radii. It is not difficult to know from the design of the oblique perforation scheme that its excellent results can be naturally extended to Examples 2 to 4.

[0061] Fig. 9 The image shows the flow pattern of oxygen breaking through the porous transmission layer to the flow channel when the center of the oblique perforation is 100 microns away from the oxygen generation center and the perforation diameter is 110 microns. The red part represents the oxygen flow and the blue part represents liquid water. Fig. 9 Shown: With Figure 2 Unlike the situation in (b) where oxygen is severely accumulated under the ribs, oxygen can smoothly enter the flow channel from the generation position through the oblique perforations, avoiding the retention of oxygen in the porous transport layer, which is beneficial for liquid water to continuously enter the porous transport layer and reach the catalytic layer to participate in the electrolysis reaction, promoting the continuous progress of the electrochemical reaction and avoiding the occurrence of local hot spots and water starvation.

[0062] Fig.10 The image shows the flow pattern of oxygen breaking through the porous transmission layer to the flow channel when the center of the oblique perforation is 100 microns away from the oxygen generation center and the perforation diameter is 120 microns. The red part represents the oxygen flow and the blue part represents liquid water. Fig.10 Shown: With Fig. 9 Similar to the case of , oxygen can smoothly enter the flow channel from the generation position through the oblique through hole, avoiding the oxygen being trapped in the porous transmission layer under the rib plate due to the obstruction of the rib plate. In addition, it can be found that when the aperture increases, the oblique through hole can accommodate more oxygen to pass through; however, since the aperture represents a low resistance path in both cases, that is, oxygen tends to flow into the flow channel from the oblique through hole, the increase in aperture does not have much effect on the oxygen flow pattern.

[0063] Fig.11 The image shows the flow pattern of oxygen breaking through the porous transmission layer to the flow channel when the center of the oblique perforation is 190 microns away from the oxygen generation center and the perforation diameter is 120 microns. The red part represents the oxygen flow and the blue part represents liquid water. Fig.11 Shown: With Fig. 9 and Fig.10 The flow conditions are similar to those of the catalyst layer. The oxygen generated on the catalyst layer can be discharged smoothly through the oblique holes, rather than Figure 2 As shown in (b), oxygen is trapped under the ribs, causing serious oxygen accumulation. Since the oblique perforations in this case are farther away from the oxygen generation position, the oxygen flow has to extend more widely in the porous transmission layer to find the oblique perforations and then enter the flow channel from the oblique perforations.

[0064] Fig.12 The curves showing the average oxygen saturation in the porous transport layer changing with time at different oblique perforation positions and diameters are shown. Fig.12It can be seen that when there is no oblique perforation, the average oxygen saturation in the porous transport layer continues to increase, reflecting the continuous accumulation of oxygen in the porous transport layer due to the obstruction of the bipolar plate ribs; and when the oblique perforation scheme is adopted, the average oxygen saturation in the porous transport layer can be steadily maintained at a low level (about 10%), reflecting the superiority of the oblique perforation scheme of the porous transport layer; in addition, it can be known that when the diameter of the oblique perforation is larger and the perforation position is closer to the oxygen generation position, the average oxygen saturation in the porous transport layer is smaller, that is, the oxygen removal effect is better. Therefore, when oxygen is generated uniformly in the entire catalytic layer plane, increasing the number of oblique perforations can make the average "oxygen-pore" distance smaller, thereby achieving a better degassing effect.

[0065] Fig.13 The curves showing the average escape velocity of oxygen in the porous transport layer changing with time at different oblique perforation positions and diameters are shown. Fig.13 It can be seen that, in general, the use of oblique perforations can make oxygen obtain a greater average escape velocity in the porous transport layer, that is, a higher degassing efficiency; in addition, it can be known that when the diameter of the oblique perforations is larger and the perforation position is closer to the oxygen generation position, the corresponding average oxygen escape velocity is also greater, that is, the oxygen removal effect is better. Therefore, when oxygen is generated uniformly in the entire catalytic layer plane, increasing the number of oblique perforations can make the average "oxygen-pore" distance smaller, thereby achieving a better degassing effect.

[0066] In summary, the oblique perforation technology and manufacturing method for the porous transport layer of the proton exchange membrane electrolyzer in the present invention have the following advantages: simple process, significant exhaust effect, help to improve the mass transfer effect, reduce concentration overpotential, improve hydrogen production efficiency, adapt to high current density operating environment, and freely adapt to different types of flow channel structures. It is very suitable for application in high current density proton exchange membrane electrolyzer equipment and has very broad technical prospects and economic benefits.

[0067] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. An obliquely perforated porous transport layer in a proton exchange membrane electrolyzer, It is characterized in that The two ends of the oblique perforations of the oblique perforated porous transport layer face the bipolar plate and the catalyst layer respectively, wherein the end facing the bipolar plate is connected to the flow channel, and the end facing the catalyst layer is located directly below the bipolar plate rib.

2. The obliquely perforated porous transport layer in the proton exchange membrane electrolyzer according to claim 1, It is characterized in that The manufacturing methods of the oblique perforations include mechanical perforation, jet perforation and laser perforation.

3. The obliquely perforated porous transport layer in the proton exchange membrane electrolyzer according to claim 2, It is characterized in that The steps of the mechanical perforation method include: cleaning the original porous transport layer and trimming its surface; determining the area on the porous transport layer that contacts the bipolar plate flow channel, and marking the position of the oblique perforation according to the oblique perforation scheme; at the oblique perforation position, according to the thickness of the porous transport layer and the flow channel-rib plate distribution, determining the diameter and angle of the oblique perforation, so that the two ends of the oblique perforation are respectively located at the flow channel section facing the bipolar plate and the rib plate section facing the catalyst layer; using a drill bit to obliquely drill holes in the porous transport layer or using a reamer to obliquely ream the porous transport layer to form holes.

4. The obliquely perforated porous transport layer in the proton exchange membrane electrolyzer according to claim 2, It is characterized in that The steps of the jet perforation method include: cleaning the original porous transport layer and trimming its surface; determining the area on the porous transport layer that contacts the bipolar plate flow channel, and marking the position of the oblique perforation according to the oblique perforation scheme; at the oblique perforation position, according to the thickness of the porous transport layer and the flow channel-rib plate distribution, determining the diameter and angle of the oblique perforation, so that the two ends of the oblique perforation are respectively located at the flow channel section facing the bipolar plate and the rib plate section facing the catalyst layer; using high-speed jet abrasive particles or water flow to impact the surface of the porous transport layer to form holes.

5. The obliquely perforated porous transport layer in the proton exchange membrane electrolyzer according to claim 2, It is characterized in that The steps of the laser perforation method include: cleaning the original porous transport layer and trimming its surface; determining the area on the porous transport layer that contacts the bipolar plate flow channel, and marking the position of the oblique perforation according to the oblique perforation scheme; at the oblique perforation position, according to the thickness of the porous transport layer and the flow channel-rib plate distribution, determining the diameter and angle of the oblique perforation, so that the two ends of the oblique perforation are respectively located at the flow channel section facing the bipolar plate and the rib plate section facing the catalyst layer; using a laser beam to irradiate the surface of the porous transport layer to form holes.

6. The obliquely perforated porous transport layer in the proton exchange membrane electrolyzer according to claim 1, It is characterized in that For the serpentine flow channel proton exchange membrane electrolyzer, an oblique perforation scheme is adopted for the porous transport layer: from the surface of each serpentine flow channel section on one side of the bipolar plate, along the flow direction, oblique holes are opened in sequence toward the corresponding rib plate section on the catalyst layer side.

7. The obliquely perforated porous transport layer in the proton exchange membrane electrolyzer according to claim 1, It is characterized in that For the parallel flow channel proton exchange membrane electrolyzer, the porous transport layer adopts an oblique perforation scheme in which oblique holes are opened from the surface of each parallel flow channel section on one side of the bipolar plate, along the flow direction, in sequence toward the corresponding rib plate section on the catalyst layer side.

8. The obliquely perforated porous transport layer in the proton exchange membrane electrolyzer according to claim 1, It is characterized in that For the interdigitated channel proton exchange membrane electrolyzer, the porous transport layer adopts an oblique perforation scheme in which oblique holes are opened in sequence along the flow direction from the surface of each parallel channel section connected to the outlet manifold on one side of the bipolar plate to the corresponding rib plate section on the catalyst layer side.

9. The obliquely perforated porous transport layer in the proton exchange membrane electrolyzer according to claim 1, It is characterized in that For the serpentine-parallel mixed flow channel proton exchange membrane electrolyzer, an oblique perforation scheme is adopted for the porous transport layer: from the surface of each serpentine flow channel section on one side of the bipolar plate, along the flow direction, oblique holes are opened in sequence toward the corresponding rib plate section on the catalyst layer side.

10. Use of the obliquely perforated porous transport layer in a proton exchange membrane electrolyzer according to any one of claims 1 to 9 in a proton exchange membrane electrolyzer.

Citation Information

Patent Citations

  • Novel anode diffusion layer and proton exchange membrane water electrolysis cell

    CN114540851A

  • Runner with vertical channel applied to electrolytic tank or fuel cell

    CN117096371A

  • Porous transmission layer containing Tesla structure

    CN117127198A

  • Membrane-electrode assembly for solid polymer electrolyte fuel cell

    JP2008071566A