Iron-doped cobalt phosphate methanol electrooxidation catalyst as well as preparation method and application thereof

By doping iron in cobalt phosphate, Fe-CoPO catalyst was prepared, which solved the problems of high working potential and low selectivity of methanol electrooxidation catalysts, and achieved low cost, high selectivity and stable formate production, which broadened its Potential for use in industrial applications.

CN119082780APending Publication Date: 2024-12-06EAST CHINA UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411185735.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the prior art, methanol electrooxidation catalysts have problems with high working potential, low selectivity and poor stability, resulting in high production cost of formate and cumbersome catalyst preparation.

Method used

Doping iron in cobalt phosphate by one-step hydrothermal method, adjusting the iron content to improve the electrocatalytic activity of methanol electrooxidation reaction, and preparing iron-doped cobalt phosphate (Fe-CoPO) catalyst to achieve low working potential and high selection sex.

Benefits of technology

The Fe-CoPO catalyst has a working potential drop to 1.436V at a current density of 100mA cm-2, maintaining high selectivity and stability, and the formate selectivity is above 97%. It is suitable for industrial applications, and its preparation method is simple and the cost is low. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082780A_ABST
    Figure CN119082780A_ABST
Patent Text Reader

Abstract

The invention discloses an iron-doped cobalt phosphate methanol electrooxidation catalyst as well as a preparation method and application thereof. The preparation method comprises the following steps: S1, carrying out ultrasonic cleaning on foamed nickel; s2, dissolving disodium hydrogen phosphate dodecahydrate and hexadecyl trimethyl ammonium bromide in a mixed solution of water and ethylene glycol, and stirring; cobalt nitrate hexahydrate and ferric nitrate nonahydrate are added, stirring is carried out, a precursor solution is obtained, and the ratio of the amount of substance of Co (NO) 2 to the amount of substance of Fe (NO3) 3 is 3.5: (0.1-3); s3, soaking the foamed nickel into the precursor solution, and refrigerating at low temperature overnight; and S4, transferring into a hydrothermal reactor, keeping at 140-180 DEG C for 8-12 hours, cooling, washing and drying to obtain the product. The iron-doped cobalt phosphate methanol electrooxidation catalyst is prepared for the first time, the working potential is as low as 1.436 V under the current density of 100 mA cm <-2 >, and the iron-doped cobalt phosphate methanol electrooxidation catalyst has remarkable advantages and application potential in methanol electrooxidation reaction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of electrocatalysts, and more specifically to an iron-doped cobalt phosphate methanol electro-oxidation catalyst and a preparation method and application thereof. Background Art

[0002] In recent years, the research on producing hydrogen by electrocatalytic reduction of abundant water resources has received extensive attention to cope with climate and environmental changes and solve energy shortages. However, the anode oxygen evolution reaction corresponding to the cathode reduction reaction requires continuous intermediate valence change steps, which makes the catalytic cycle kinetics complex and the overall catalytic kinetics slow. In recent years, the oxygen evolution reaction is replaced by thermodynamically more favorable small molecule oxidation reactions (methanol, glucose, furfuryl alcohol, etc.), coupled with cathode reduction reactions (such as hydrogen evolution reaction, CO2 reduction reaction), so as to achieve the purpose of improving the utilization rate of electric energy and obtaining high value-added anode products.

[0003] At present, 80% of formic acid in industry is produced by methyl formate hydrolysis. This process produces methyl formate through carbonylation of methanol and toxic and explosive CO, and then hydrolyzes it to formic acid at high temperature (413K) and high pressure (4MPa). In contrast, obtaining formate through methanol selective electrooxidation (MOR) overcomes the disadvantages of high temperature, high pressure and high energy consumption required for industrial production of formic acid, and is a very promising method for producing formic acid. The key to the electrocatalytic oxidation of methanol to formic acid is the degree of methanol oxidation. However, most methanol oxidation reaction (MOR) electrocatalysts completely oxidize methanol to carbon dioxide, resulting in relatively serious carbon emissions. At present, a variety of electrocatalysts have been developed, such as precious metal-based electrocatalysts platinum (Pt), palladium (Pd) and ruthenium (Ru), but these catalysts cannot provide selective conversion of methanol to formate, and as mentioned above, precious metal-based catalysts are scarce on the earth and expensive, and cannot provide power for the methanol economy. Recently, some non-precious transition metal-based electrocatalysts have been widely studied for selective methanol formate, especially nickel (Ni)-based catalysts and cobalt (Co)-based catalysts. However, the working potential of non-precious metal catalysts that can be used for efficient electrocatalytic oxidation of methanol to formate is relatively high. Therefore, it is an urgent need to develop MOR catalysts with good catalytic activity and selectivity.

[0004] At present, in the existing technology, the disadvantages of precious metal catalysts are mainly concentrated in high cost, poor formate selectivity, high cost of electrosynthesis of formic acid, and cumbersome catalyst preparation. The development of transition metal-based electrocatalysts can effectively reduce the cost of catalysts and has made initial progress, but their catalytic activity is still lower than that of precious metal catalysts, and a higher working potential (>1.5V, compared with reversible hydrogen electrodes) is required to reach industrial current density (100mA cm -2). The relatively high working potential limits their practical application in the electrosynthesis of formic acid. In addition, the stability of non-precious metal catalysts is poor because the catalyst loaded on the working electrode dissolves into the electrolyte during the electrooxidation process. Therefore, it is necessary to develop a methanol electrooxidation catalyst with low working potential, high selectivity, and high stability, and further clarify the source of activity in the material. Summary of the invention

[0005] The purpose of the present invention is to provide an iron-doped cobalt phosphate methanol electro-oxidation catalyst and a preparation method and application thereof, so as to solve the problem that the prior art lacks a methanol electro-oxidation catalyst with low working potential, high selectivity and high stability.

[0006] According to a first aspect of the present invention, a method for preparing an iron-doped cobalt phosphate methanol electro-oxidation catalyst is provided, comprising the following steps: S1, ultrasonically cleaning the nickel foam with an acetone:HCl solution of 1:1, ethanol and deionized water, respectively, and then drying to remove impurities on the surface of the nickel foam; S2, dissolving disodium hydrogen phosphate dodecahydrate and hexadecyltrimethylammonium bromide in a mixed solution of water and ethylene glycol at a molar ratio of 3:1 and magnetically stirring; then, adding cobalt nitrate hexahydrate and iron nitrate nonahydrate thereto, stirring to obtain a light pink precursor solution, wherein The molar ratio of Co(NO)2 to Fe(NO3)3 is 3.5:(0.1-3); S3, immersing the pre-cleaned nickel foam into the light pink precursor solution and refrigerating overnight at low temperature to allow the iron-doped cobalt phosphate to crystallize rapidly on the surface of the nickel foam and grow nano-flower crystals; S4, transferring the mixture obtained in step S3 into a Teflon hydrothermal reactor, maintaining it at 140-180°C for 8-12 hours, naturally cooling it to room temperature, rinsing it with deionized water, and then drying it in an oven to obtain an iron-doped cobalt phosphate methanol electro-oxidation catalyst.

[0007] Preferably, step S1 comprises: ultrasonically cleaning the nickel foam for 5 minutes using acetone:HCl=1:1 solution, ethanol and deionized water respectively, and then drying at 60° C. for 10 to 14 hours.

[0008] Preferably, in step S2, the molar ratio of Co(NO)2 to Fe(NO3)3 is 3.5:(0.5-2).

[0009] Preferably, step S3 comprises: refrigerating at 0-8°C overnight.

[0010] Preferably, in step S4, the closed reaction container is heated to allow the compounds in the solvent to undergo a chemical reaction under specific temperature and pressure conditions, thereby synthesizing iron-doped cobalt phosphate Fe-CoPO.

[0011] According to the preparation method provided by the present invention, the purpose of step S1 is to remove surface oxide impurities. This step is a general method for treating nickel foam and has been academically reported; the role of step S2 is to prepare a light pink precursor solution to facilitate the subsequent preparation of iron-doped cobalt phosphate; the role of step S3 is to allow iron-doped cobalt phosphate to crystallize rapidly on the surface of nickel foam at low temperature to grow nanoflower crystals; step S4 heats the closed reaction container to allow the compounds in the solvent to react chemically under specific temperature and pressure conditions, thereby synthesizing iron-doped cobalt phosphate Fe-CoPO.

[0012] According to a second aspect of the present invention, there is provided an iron-doped cobalt phosphate methanol electro-oxidation catalyst prepared according to the above preparation method, which has a high conductivity at 100 mA cm -2 At a current density of , the working potential is as low as 1.436V.

[0013] According to a third aspect of the present invention, there is provided a use of an iron-doped cobalt phosphate methanol electro-oxidation catalyst in methanol electro-oxidation.

[0014] Preferably, the divalent and trivalent cobalt oxygen bonds in cobalt tetroxide formed by electrochemical reconstruction of iron-doped cobalt phosphate are active sites for the selective electrocatalytic oxidation of methanol to high-value-added formic acid.

[0015] According to a preferred embodiment of the present invention, a method for preparing an iron-doped cobalt phosphate methanol electro-oxidation catalyst is provided, comprising the following steps: Step 1: removing impurities on the surface of nickel foam: firstly, using acetone: HCl = 1: 1 solution, ethanol and deionized water to remove (1×1 cm 2 ) Nickel foam (NF) was ultrasonically cleaned for 5 minutes and dried at 60°C for 12 hours; Step 2: 1.074g (3mmol) of disodium hydrogen phosphate dodecahydrate and 0.364g (1mmol) of hexadecyltrimethylammonium bromide were dissolved in a mixed solution of 20mL of water and ethylene glycol (3:2) and magnetically stirred for 5 minutes. Subsequently, 0.873g (3mmol) of cobalt nitrate hexahydrate and a certain amount (0.1-3mmol, changed according to the specific application) of iron nitrate nonahydrate were added to the above solution, and stirring was continued for 20 minutes to obtain a light pink precursor solution; Step 3: The pre-cleaned nickel foam was immersed in the above mixed solution and refrigerated at 0-8°C overnight; Step 4: The mixture was transferred into a 150mL Teflon hydrothermal reactor and kept at 160-180°C for 10 hours. After cooling naturally to room temperature, the sample was thoroughly rinsed with deionized water and then dried in an oven at 60°C for 12 hours.

[0016] As described in the background technology section of the present invention, on the one hand, the disadvantages of noble metal catalysts are mainly concentrated in high cost, poor formate selectivity, high cost of electrosynthesis of formic acid, and cumbersome preparation. On the other hand, the development of transition metal-based electrocatalysts can effectively reduce the cost of catalysts and has made initial progress, but their catalytic activity is still lower than that of noble metal catalysts, and a higher working potential (>1.5V, compared with reversible hydrogen electrodes) is required to reach industrial current density (100mA cm -2 ).

[0017] In view of the shortcomings of methanol electro-oxidation catalysts in the prior art, such as high working potential, poor methanol selectivity, and poor stability, the present invention provides an iron-doped cobalt phosphate methanol electro-oxidation catalyst and its preparation and application, which uses a one-step hydrothermal method to change the electrocatalytic activity of the methanol electro-oxidation reaction by simply changing the content of doped iron in cobalt phosphate. Subsequently, in the corresponding electrochemical test, we found that doping a specific proportion of iron in cobalt phosphate can reduce the working potential and improve the methanol selectivity and stability of the methanol electro-oxidation reaction.

[0018] The key inventive points of the present invention are as follows:

[0019] 1) The present invention shows significant performance improvement by doping a certain amount of iron (Fe) into cobalt phosphate (CoPO). Specifically, the Fe-CoPO electrocatalyst has a high conductivity at 100 mA cm -2 The working potential is 1.436 V at a current density of 100 mA cm -2 The selectivity of formate was maintained above 97% at a current density of 200 and 300 mA cm for 16 h. -2 The formate selectivity was 100% at the current density of 1.

[0020] 2) The present invention provides a simpler, lower-cost and large-scale production method for preparing methanol electro-oxidation catalyst by doping CoPO with an appropriate amount of Fe, i.e., doping with iron according to the molar ratio of Co(NO)2:Fe(NO3)3=3.5:(0.1-3), thereby promoting the popularization of methanol electro-oxidation technology in industrial applications. On the contrary, if the amount of iron nitrate added is too high, the electrochemical performance of the prepared methanol electro-oxidation catalyst will decrease, i.e., reaching 100mA cm -2 The required voltage rises and cannot meet the demand.

[0021] 3) The Fe-CoPO catalyst prepared by the method of the present invention was tested by in situ Raman spectroscopy to prove that the divalent and trivalent cobalt oxygen bonds (Co 2 / 3+-O) is the active site for the selective electrocatalytic oxidation of methanol to high value-added formic acid.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1) Compared with other non-precious metal catalysts for methanol electrooxidation, Fe-CoPO showed significant performance improvement in methanol oxidation. -2 The working potential is 1.436 V at a current density of 100 mA cm-1, which solves the problems of low current density, high working potential, poor formate selectivity and poor stability of other non-precious metal catalysts in methanol electrooxidation. Fe-CoPO has excellent formate selectivity and stability: at 100 mA cm-1, -2 The selectivity of formate was maintained above 97% at a current density of 200 and 300 mA cm for 16 h. -2 The reactors were operated for 8 hours at current densities of 1.3 and 1.5 respectively, and the formate selectivity was 100%.

[0024] 2) The present invention proposes to dope iron to optimize the deficiencies of cobalt phosphate in the performance of methanol electro-oxidation reaction, such as low current density, high working potential and poor formate selectivity. Compared with other methods to solve this problem, such as constructing a multi-metal structure or nanoparticle modification, the preparation method of the present invention is simpler, has low raw material cost, and can be mass-produced, thereby making methanol electro-oxidation technology easier to implement in industrial applications.

[0025] 3) The divalent cobalt oxygen bond (Co) in cobalt phosphate tetrahydrate (Co3(PO4)2·4H2O) prepared by hydrothermal synthesis 2+ -O) tends to reconstruct the tetravalent cobalt oxygen bond (Co-O) in cobalt tetraoxide (CoO2) during the selective electrooxidation of methanol. 4+ -O) bond, however, when iron is incorporated into cobalt phosphate, the divalent cobalt oxygen bond (Co 2+ -O) prefers to reconstruct the divalent and trivalent cobalt oxygen bonds (Co3O4) in cobalt tetroxide (Co3O4). 2 / 3+ -O). The present invention firstly finds that divalent and trivalent cobalt oxygen bonds are active sites for the selective electro-oxidation reaction of methanol, which is beneficial to the selective oxidation of methanol to formic acid.

[0026] In summary, the present invention prepares for the first time such an iron-doped cobalt phosphate methanol electrooxidation catalyst by doping a certain amount of Fe into CoPO during the synthesis process, that is, controlling the molar ratio of Co(NO)2 to Fe(NO3)3 to 3.5:(0.1-3). -2At a current density of , the working potential is as low as 1.436 V. The relatively low working potential broadens the practical application of the iron-doped cobalt phosphate methanol electro-oxidation catalyst in the electrosynthesis production of formic acid, making the iron-doped cobalt phosphate methanol electro-oxidation catalyst of the present invention have significant advantages and application potential in the methanol electro-oxidation reaction. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 Scanning electron microscope images of the Fe-CoPO electrocatalyst (a) and the CoPO electrocatalyst (b) prepared in Example 1 of the present invention;

[0028] Figure 2 Linear sweep voltammograms of electrocatalysts Fe-CoPO and CoPO control;

[0029] Figure 3 The double layer capacitance curves of the electrocatalysts Fe-CoPO and CoPO are compared;

[0030] Figure 4 (a) The chronopotentiometry curve of Fe-CoPO electrocatalyst and its formate selectivity graph (b);

[0031] Figure 5 In-situ Raman curve of CoPO electrocatalyst;

[0032] Figure 6 is the in-situ Raman curve of Fe-CoPO electrocatalyst;

[0033] Figure 7 The chronopotentiometry curves of the electrocatalysts Fe-CoPO and CoPO (a) and their formate selectivity (b);

[0034] Figure 8 The linear sweep voltammetry curves of the electrocatalyst prepared by using different molar numbers of ferric nitrate in Example 2 of the present invention and the Fe-CoPO electrocatalyst prepared in Example 1 are compared. DETAILED DESCRIPTION

[0035] The present invention will be further described below in conjunction with specific examples. It should be understood that the following examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. Unless otherwise specified, the technical means used in the examples are conventional operations in the art, or according to the experimental methods recommended by the instrument and equipment manufacturers. The reagents and materials used in the examples can be obtained from commercial sources unless otherwise specified.

[0036] Example 1

[0037] The reagents used in the iron-doped cobalt phosphate of the present invention are all analytically pure and purchased from Sinopharm Chemical Reagent Co., Ltd. A specific preparation process of an iron-doped cobalt phosphate methanol electro-oxidation catalyst is as follows:

[0038] 1. First, use acetone: HCl = 1:1 solution, ethanol and deionized water to treat the nickel foam (1×1cm 2 ) The oxide impurities on the surface were ultrasonically cleaned for 5 minutes and dried at 60°C for 12 hours.

[0039] 2. First, 1.074 g (3 mmol) of disodium hydrogen phosphate dodecahydrate and 0.364 g (1 mmol) of hexadecyltrimethylammonium bromide were dissolved in a mixed solution of 20 mL of water and ethylene glycol (3:2) and magnetically stirred for 5 min. Subsequently, 0.873 g (3 mmol) of cobalt nitrate hexahydrate and 0.606 g (1.5 mmol) of iron nitrate nonahydrate were added to the above solution and stirred for 20 min to obtain a light pink precursor solution.

[0040] 3. Immerse the pre-cleaned nickel foam in the above mixed solution and refrigerate overnight.

[0041] 4. The mixture was transferred into a 150 mL Teflon hydrothermal reactor and maintained at 160 °C for 10 h. After cooling naturally to room temperature, the sample was thoroughly rinsed with deionized water and then dried in an oven at 60 °C for 12 h.

[0042] The obtained samples were named according to whether they were doped with iron in step 2. The sample without iron nitrate nonahydrate was named cobalt phosphate (referred to as CoPO), and the sample doped with iron nitrate nonahydrate was named iron-doped cobalt phosphate (Fe-CoPO).

[0043] Electrochemical testing and product analysis of methanol electro-oxidation catalysts:

[0044] Electrolysis reaction was carried out using a single-cell electrolytic cell: Methanol electrooxidation reaction was tested in a three-electrode system using a CHI electrochemical workstation (model 660e). The above-mentioned cobalt iron phosphate electrode was used as the working electrode, alcohols were used as reaction substrates dissolved in an alkaline aqueous solution as the electrolyte, a platinum sheet electrode was used as the counter electrode, and the reference electrode was an Ag / AgCl electrode. Electrocatalytic selective oxidation reaction was carried out at room temperature of 25-30°C to generate high value-added formic acid. Cyclic voltammetry was performed at 50mV s -1 The scan rate was 5 mV s -1 All polarization curves recorded were not iR corrected and converted to the reversible hydrogen electrode scale by the following equation: E (relative to RHE) = E + 0.059 × pH + E Ag / AgCl

[0045] Where E Ag / AgCl 0.1976 V relative to RHE, pH 14.

[0046] The calculation formula of Tafel slope is: η=a+b×log(j)

[0047] Here, η, b, and j represent the overpotential, Tafel slope, and current density, respectively.

[0048] The calculation formula of double layer capacitance (Cdl) is as follows: C dl =Δ j / 2 / V

[0049] where Δj is the difference between the anode and cathode current densities at open circuit voltage.

[0050] Electrochemical impedance spectroscopy was performed at open circuit voltage with a frequency of 0.01 Hz to 100 kHz and an amplitude of 10 mV. Chronopotentiometry was used to evaluate the long-term performance of the electrocatalyst.

[0051] Raman test: In-situ Raman spectroscopy was performed on a Horiba LABRAM HR Raman spectrometer. Platinum wire was used as the counter electrode, Ag / AgCl was used as the reference electrode, and the K004 in-situ Raman test cell ( Figure 1 ) were used for in situ experiments. The excitation wavelength was 532 nm, and a 50× microscope objective with a numerical aperture of 0.55 was used. The spectra of the pretreated electrodes were collected at each applied potential for 60 seconds.

[0052] The content of the methanol oxidation reaction product was analyzed by nuclear magnetic resonance (NMR, Avance III 400 instrument (Bruker)). First, a series of formic acid (HCOOH) solutions with different concentrations (0.5 mmol / L, 1 mmol / L, 5 mmol / L, 10 mmol / L, 50 mmol / L, 100 mmol / L, 200 mmol / L) were prepared. 500 μL of formic acid solution and 100 μL of heavy water were added to the NMR tube and mixed thoroughly for NMR testing. A standard curve was drawn based on the proportional relationship between the formate ion signal peak integral intensity and the formate ion concentration. In order to analyze the product in the electrolyte, 500 μL of electrolyte and 100 μL of heavy water were added to the NMR tube and mixed thoroughly. Then the NMR test was performed to obtain the comprehensive intensity of the synthetic ion signal. The content of formate was calculated based on the standard curve. The calculation formula of the Faraday efficiency is as follows: (Formate selectivity) Faraday efficiency = N × F × n / Q = N × F × n / (I × t)

[0053] Where N is the number of moles of product generated, N is the number of moles of formic acid generated, F is the Faraday constant, I is the applied current, and t is the electrolysis time.

[0054] The morphology of the Fe-CoPO and CoPO electrodes prepared above was characterized.

[0055] like Figure 1 , SEM image of CoPO without Fe doping (see Figure 1 In contrast, the scanning electron microscopy (SEM) image of Fe-CoPO (see Figure 1 Figure b) clearly shows that the nickel foam skeleton is wrapped by a uniformly distributed catalytic layer, and the crystalline nanoparticles are embedded in the pores of the nickel foam. This structure presents a hierarchical pore structure with coexistence of mesopores and macropores, and the catalytic layer is evenly distributed. This structure not only provides more active sites for methanol electro-oxidation reaction, but also helps the diffusion and transport of substances. By comparison, it was found that the doping of Fe helps CoPO to reconstruct on the surface of nickel foam and form a relatively stable surface composition and structure.

[0056] The Fe-CoPO and CoPO electrodes prepared above were subjected to electrochemical tests.

[0057] like Figure 2 , for CoPO catalyst, up to 10 mA cm -2 The potential required for the current density is 1.382 V. Incorporation of trace amounts of iron into CoPO significantly reduces the potential of CoPO from 1.382 V to 1.284 V (Fe-CoPO), a decrease of 98 mV. -2 Under the current density, Fe-CoPO has the lowest potential of 1.436 V, which is much lower than CoPO (1.504 V) and nickel foam (1.597 V).

[0058] like Figure 3 We measured the electrochemical double layer capacitance (C dl ) to compare the performance of Fe-CoPO and CoPO. dl The Cdl value of Fe-CoPO was found to be 4.42 mF cm -2 , while CoPO's C dl The value is 1.18mF cm -2. This indicates that Fe-CoPO has a larger electrochemical specific surface area, which means that there are more active sites on the Fe-CoPO electrode. Based on these experimental results, we can infer that the improvement in the activity of methanol electrooxidation reaction is mainly due to two aspects. First, the electrochemically active interface generated by the heterostructure between Fe and Co on the Fe-CoPO electrode plays an important role in the catalysis of the reaction. Second, the increase in the electrochemical specific surface area after doping Fe in Fe-CoPO produces more active sites.

[0059] The selective methanol electrooxidation reaction of Fe-CoPO and CoPO was tested by chronopotentiometry.

[0060] like Figure 4 We used chronopotentiometry to test the selective methanol electrooxidation reaction of Fe-CoPO. The results showed that Fe-CoPO -2 The electrode was operated at a current density of 200 mA cm for at least 16 h, with the oxidation potential of the electrode increasing by only 20 mV, demonstrating its excellent long-term stability. In addition, electrolyte samples were collected regularly and the selectivity for formate was measured by NMR analysis. The selectivity for formate was approximately 100% during methanol electrooxidation. Even at higher current densities (e.g., 200 mA cm -2 or 300mA cm -2 ), Fe-CoPO still maintains excellent stability. It is worth noting that even at 300 mA cm -2 Even at high current density, Fe-CoPO can still maintain the selectivity of formate at 100%.

[0061] like Figure 5 , we performed in situ Raman spectroscopy analysis of CoPO. Under open circuit potential (OCPT) conditions, the CoPO sample showed several Raman scattering modes, located at 437.5 cm -1 、504.4cm -1 and 684.8cm -1 These diffraction peaks can be attributed to the bonding vibration modes in different species. Specifically, 437.5 cm -1 The peak at can be attributed to the Co 4+ -O key E g Vibration mode, 504.4cm -1 The peak at can be attributed to the Co in cobalt oxyhydroxide (CoOOH). 3+ -O key E g Vibration mode, and 684.8cm -1 The peak at can be attributed to the Co in Co3O4 2 / 3+ -O key A 1gSymmetric mode. In the in situ Raman spectrum, we observed that the CoPO sample has a peak at 437 cm -1 The peak at 20° gradually increases with the applied potential. This indicates that the Co 4+ The content of -O bonds increases, which also indicates the deepening of the reconstruction degree.

[0062] like Figure 6 , we performed in situ Raman spectroscopy analysis of Fe-CoPO. However, we were unable to detect Co in the CoO2 species in the Raman spectrum of Fe-CoPO. 4+ In contrast, as the applied voltage increases from 1.03 V to 1.63 V, we observe that Co 2 / 3+ The characteristic peak of -O bond gradually increases. This finding indicates that Co 2 / 3+ The -O bond may be the active site for methanol electrooxidation.

[0063] like Figure 7 , in order to verify Co 2 / 3+ Based on the hypothesis that the -O bond is the active site of the methanol electrooxidation reaction, we used chronopotentiometry to test the selective methanol electrooxidation reaction of Fe-CoPO and CoPO for 12 hours. The experimental results show that Fe-CoPO exhibits 100% formate selectivity, while the formate selectivity of CoPO is only 39.7%. This indicates that Fe-CoPO has higher selectivity and activity in the methanol electrooxidation reaction. During the methanol electrooxidation reaction, Co in CoO2 formed by electrochemical reconstruction of CoPO 4+ -O bonds are believed to have excellent catalytic activity for oxygen evolution reaction. - The ions will attack the Co 4+ -O bond, forming an intramolecular OO bond, and then forming O2, thereby promoting the oxygen evolution reaction. 2 / 3+ -O bonds promote the formation of formate. In summary, based on the experimental results, we conclude that Co 2 / 3+ -O bonds are assumed to be the active sites for methanol electrooxidation. The Fe-CoPO catalyst forms Co3O4 and Co 2 / 3+ -O bond, showing higher selectivity and activity in methanol electrooxidation.

[0064] Example 2

[0065] Iron-doped cobalt phosphate methanol electrooxidation catalysts prepared using different molar amounts of iron nitrate:

[0066] The specific method is the same as that of Example 1, except that the doping amounts of iron nitrate are 0.5 mmol, 1 mmol, 2 mmol, and 3 mmol, respectively, and the other steps remain unchanged.

[0067] The electrochemical performance of the electrocatalyst prepared in Example 2 in the methanol electrooxidation reaction was tested in the same manner as in Example 1. The test results are shown in FIG. Figure 8 The electrochemical activity test of the electrocatalyst prepared using different molar numbers of iron nitrate showed that the activity was not much different from that of the iron-doped cobalt phosphate electrocatalyst prepared in Example 1.

[0068] Example 3

[0069] In this example, the catalytic performance of the Fe-CoPO / NF methanol electro-oxidation catalyst prepared by the present invention is compared with that of other catalysts previously reported in the literature. The results are shown in Table 1 below. Table 1. Comparison of electrocatalytic performance of different catalysts [1] K.Xiang, D.Wu, X.Deng, M.Li, S.Chen, P.Hao, X.Guo, J.-L.Luo, FunctionalMaterials,2020 Mar,30(10). [2] J.Li, Z.Luo, F.He, Y.Zuo, C.Zhang, J.Liu, ofMaterials Chemistry A,2018Dec 7,6(45):22915-22924. [3]M.G.Siahroudi,A.A.Daryakenari,Y.B.Molamahaleh,Q.Cao,M.A.Daryakenari,J.J.Delaunay,H.Siavoshi,F.Molaei.Ethylene glycol assistedsolvo-hydrothermal synthesis of NGr-Co3O4 nanostructures for ethanolelectrooxidation[J].International Journal of Hydrogen Energy,2020 Nov 6,45(55):30357-30366. [4]W.Wang,Y.-B.Zhu,Q.Wen,Y.Wang,J.Xia,C.Li,M.-W.Chen,Y.Liu,H.Li,H.-A.Wu,T.Y.Zhai.Modulation of Molecular Spatial Distribution and Chemisorptionwith PerforatedNanosheets for Ethanol Electro-oxidation[J].AdvancedMaterials,2019 Jul,31(28). [5]T.Mushiana,M.Khan,M.I.Abdullah,N.Zhang,M.Ma.Facile sol-gelpreparation of high-entropy multielemental electrocatalysts for efficientoxidation of methanol and urea[J].NanoResearch,2022 Jun,15(6):5014-5023. [6]B.Zhao,J.-W.Liu,Y.-R.Yin,D.Wu,J.-L.Luo,X.-Z.Fu.Carbon nanofibers@NiSecore / sheath nanostructures as efficient electrocatalysts for integratinghighly selective methanol conversion and less-energy intensive hydrogenproduction[J].Journal of Materials Chemistry A,2019Dec 7,7(45):25878-25886. [7]S.Hao,M.Cong,H.Xu,X.Ding,Y.Gao.Bismuth-Based Electrocatalysts forIdentical Value-Added Formic Acid Through Coupling CO2 Reduction and MethanolOxidation[J].Small,2023.[8]S.Jiang,T.Xiao,C.Xu,S.Wang,H.-Q.Peng,W.Zhang,B.Liu,Y.-F.Song.Passivating Oxygen Evolution Activity of NiFe-LDH throughHeterostructure Engineering to Realize High-Efficiency ElectrocatalyticFormate and Hydrogen Co-Production[J].Small,2023Jul,19(27). [9]J.Hao,J.Liu,D.Wu,M.Chen,Y.Liang,Q.Wang,L.Wang,X.-Z.Fu,J.-L.Luo.Insitu facile fabrication of Ni(OH)2nanosheet arrays for electrocatalytic co-production of formate and hydrogen from methanol in alkaline solution[J].Applied Catalysis B-Environmental,2021Feb,281.

[0070] Through the above comparison, it can be determined that the iron-doped cobalt phosphate methanol electro-oxidation catalyst prepared according to the present invention has significant advantages and application potential in the methanol electro-oxidation reaction.

[0071] The above is only a preferred embodiment of the present invention, and is not intended to limit the scope of the present invention. The above embodiments of the present invention can also be modified in various ways. All simple, equivalent changes and modifications made according to the claims and the description of the present invention fall within the scope of protection of the claims of the present invention. The contents not described in detail in the present invention are all conventional technical contents.

Claims

1. A method for preparing an iron-doped cobalt phosphate methanol electro-oxidation catalyst, characterized in that: The following steps are involved: S1, ultrasonically cleaning the nickel foam with acetone:HCl=1:1 solution, ethanol and deionized water, and then drying to remove impurities on the surface of the nickel foam; S2, dissolving disodium hydrogen phosphate dodecahydrate and hexadecyltrimethylammonium bromide in a mixed solution of water and ethylene glycol at a molar ratio of 3:1 and magnetically stirring; then, adding cobalt nitrate hexahydrate and iron nitrate nonahydrate thereto, stirring to obtain a light pink precursor solution, wherein the molar ratio of Co(NO)2 to Fe(NO3)3 is 3.5:(0.1-3); S3, immersing the pre-cleaned nickel foam into the light pink precursor solution and refrigerating overnight at low temperature, so that the iron-doped cobalt phosphate rapidly crystallizes on the surface of the nickel foam to grow nano flower crystals; S4, transferring the mixture obtained in step S3 into a Teflon hydrothermal reactor, maintaining it at 140-180° C. for 8-12 hours, cooling it naturally to room temperature, rinsing it with deionized water, and then drying it in an oven to obtain an iron-doped cobalt phosphate methanol electro-oxidation catalyst.

2. The preparation method according to claim 1, characterized in that: Step S1 comprises: ultrasonically cleaning the nickel foam with acetone:HCl=1:1 solution, ethanol and deionized water for 5 minutes respectively, and then drying at 60° C. for 10 to 14 hours.

3. The preparation method according to claim 1, characterized in that: In step S2, the molar ratio of Co(NO)2 to Fe(NO3)3 is 3.5:(0.5-2).

4. The preparation method according to claim 1, characterized in that: Step S3 comprises: refrigerating at 0-8°C overnight.

5. The preparation method according to claim 1, characterized in that: In step S4, by heating the sealed reaction container, the compounds in the solvent can be chemically reacted under specific temperature and pressure conditions, thereby synthesizing iron-doped cobalt phosphate Fe-CoPO.

6. An iron-doped cobalt phosphate methanol electro-oxidation catalyst prepared according to the preparation method according to any one of claims 1 to 5, characterized in that: At 100mA cm -2 At a current density of , the working potential of the iron-doped cobalt phosphate methanol electro-oxidation catalyst is as low as 1.436V.

7. Use of the iron-doped cobalt phosphate methanol electro-oxidation catalyst as claimed in claim 6 in methanol electro-oxidation.

8. The use according to claim 7, characterized in that: The divalent and trivalent cobalt oxygen bonds in cobalt tetroxide formed by electrochemical reconstruction of iron-doped cobalt phosphate are active sites for the selective electrocatalytic oxidation of methanol to high-value-added formic acid.