Rolling and folding adjusting method for high-roughness electrolytic copper foil raw foil and product of high-roughness electrolytic copper foil raw foil
By setting annular lifting parts at both ends of the winding roller and controlling production parameters, the problem of discounting for winding of high-roughness electrolytic copper foil is solved, which significantly improves the yield rate and reduces energy waste, making it suitable for industrial production.
Patent Information
- Application Number
- CN202411211475.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
AI Technical Summary
High-roughness electrolytic copper foil is prone to discounts during the production process, resulting in energy waste and a decrease in yield. The existing technical solutions are complex and are not suitable for all electrolytic copper foils.
By setting an annular lifting piece at both ends of the winding roller, and controlling the production line speed and winding tension of the foil generator in the range of 3.7 to 4.4 m/min, 196 to 343N, combined with conventional electrolyte formulations and collagen aqueous solution additives, Significantly improved the phenomenon of discounts for collection.
It effectively reduces energy waste in the production process, improves yield, and is simple and controllable, suitable for industrial production.
Smart Images

Figure CN119082809A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of preparation of electrolytic copper foil, and in particular relates to a method for adjusting the rolling and folding of raw electrolytic copper foil with high roughness and a product thereof. Background Art
[0002] Electrolytic copper foil is an important electronic material, which is widely used in copper clad laminate (CCL), printed circuit board (PCB), lithium-ion battery manufacturing and other fields. The production of raw foil in electrolytic copper foil is carried out in the raw foil machine, including in the electrolytic cell of the raw foil machine, copper sulfate electrolyte is under the action of direct current, copper ions obtain electrons and are electro-deposited on the surface of the cathode roller to form raw foil. It includes: continuous rotation of the cathode roller, pickling, washing, drying, peeling and other processes, the copper foil is continuously peeled off, and rolled up to form a roll of raw foil. Raw foil rolling, as the end process of raw foil production, plays a vital role in the entire electrolytic copper foil production process. However, it was found in the experiment that the higher the surface roughness of the raw foil, the more likely the raw foil will be folded during the production and rolling process, resulting in energy waste in the production process and a decrease in the yield of raw foil.
[0003] Due to its unique physical properties, high-roughness copper foil has been widely used in fields including electrolytic capacitors, automotive electronics, consumer electronics, new energy vehicle power batteries, 5G communications, IDC data centers, etc. Therefore, it is urgent to solve the problems of energy waste and reduced yield caused by discounts.
[0004] A Chinese patent document with application publication number CN 114250491 A discloses a control method for reducing the folding defects caused by lithium battery copper foil during the production process, including: S1, when power is turned on, copper in the solution is deposited on the surface of the cathode roller to form copper foil, and after the copper foil rotates out of the liquid surface with the cathode roller, it is continuously peeled off from the cathode roller through a peeling roller; S2, under a given current, the copper foil passes through the passivation liquid in the passivation tank to perform anti-oxidation treatment on the copper foil; S3, the passivated copper foil is dried in an oven, and the oven is provided with an upper and lower hot air circulation system; S4, the copper foil after the drying treatment is rolled up to generate rolled copper foil. This technical solution is specifically aimed at the folding phenomenon caused by copper foil being baked in an oven. The oven is specially designed, specifically: the interior of the oven is divided into two parts, the upper part is divided into two layers, each layer has two heating lamps, the distance between the two heating lamps in the upper layer of the upper part is 4cm, the outer diameter of the lamp is 1cm, the distance between the two heating lamps in the lower layer of the upper part is 6cm, the outer diameter of the lamp is 1.5cm; the lower part is also divided into two layers, each layer has two heating lamps, the distance between the two heating lamps in the lower layer of the lower part is 4cm, the outer diameter of the lamp is 1cm, the distance between the two heating lamps in the upper layer of the lower part is 6cm, the outer diameter of the lamp is 1.5cm.
[0005] The above technical solution requires additional improvements to the oven structure, and the oven has a complex structure, unique control parameters, and poor compatibility. In addition, the above technical solution only addresses the folding phenomenon caused by the lithium battery copper foil being baked in the oven, and is not of reference value for solving the folding phenomenon caused by the high surface roughness of the raw foil. Summary of the invention
[0006] In view of the above problems, the present invention discloses a method for adjusting the rolling and folding of high-roughness electrolytic copper foil raw foil. On the basis of not adding or complicating the improvement of the original equipment, the rolling and folding phenomenon of high-roughness electrolytic copper foil raw foil with a rough surface roughness ≥4.5μm is significantly improved, and the problems of energy waste and low yield rate in the production process are effectively solved.
[0007] To achieve the above purpose, the specific technical solution of the present invention is as follows:
[0008] A method for adjusting the reeling and folding of a raw electrolytic copper foil with high roughness, comprising:
[0009] Prepare electrolyte to maintain stable production of raw foil, and then roll up the produced raw foil through a winding roller equipped with an annular heightening member;
[0010] During the production process, the production line speed of the foil machine is controlled to be 3.7-4.4 m / min and the winding tension is controlled to be 196-343 N.
[0011] There are two annular heightening members, which are symmetrically arranged at two ends of the winding roller and contact the two ends of the raw foil;
[0012] The thickness of the annular heightening member is 105-210 μm.
[0013] Aiming at the folding phenomenon of electrolytic copper foil with high roughness of 4.5 μm or more, the present invention can significantly improve the folding phenomenon of the foil during rolling without adding or complicating the original equipment, only by accurately controlling the parameters in the production process (controlling the production line speed of the foil machine to be 3.7-4.4 m / min and the winding tension to be 196-343 N), and combining with simple improvement of the winding roller (adding annular heightening parts on both sides of the winding roller), and the winding length is ≥8000 m, thereby effectively reducing the energy waste in the production process and significantly improving the yield rate.
[0014] The test found that if the production line speed and winding tension of the raw foil machine are not within the above range, and the winding roller is not raised, or the height is inappropriate, the raw foil winding length will be too short and cannot meet the minimum length requirement for post-processing (≥500). The raw foil can only be scrapped, which will cause serious waste of production energy.
[0015] The inventors have conducted detailed research on the relationship between the roughness of the rough surface of the raw foil and the continuous winding length, and concluded that the higher the roughness, the more likely it is to bend, resulting in too short a winding length. The specific relationship is shown in Table 1 below. The electrolyte compositions for producing raw foils of various roughnesses in Table 1 are all conventional formulas in the field and are not described in detail here.
[0016] Table 1
[0017]
[0018] a: The height in this table is 0, which means no simple improvement is made to the winding roller.
[0019] The annular heightening member used in the present invention may be an annular gasket, or may be directly made of scraps from the production of copper foil and wound around the surface of the winding roller to achieve the heightening effect.
[0020] Preferably, the width of the annular heightening member is 1 to 2 cm.
[0021] Further preferably, two sections of 1 cm wide strip copper foil are used as annular heightening members and are symmetrically wound around the two ends of the winding roller, ensuring contact with the two ends of the wound raw foil and that the center line along the length direction of the copper foil is flush with the edge of the raw foil.
[0022] The electrolyte in the present invention adopts conventional types in the art, as long as the roughness of the rough surface of the prepared raw foil is guaranteed to be ≥4.5 μm.
[0023] for example:
[0024] The electrolyte includes a pure electrolyte and an additive;
[0025] The raw material composition of the pure electrolyte includes: 20-110 g / L copper ions, 70-135 g / L sulfuric acid and 5-20 mg / L chloride ions;
[0026] The additive is selected from a collagen aqueous solution with a concentration of 3 to 5 g / L.
[0027] Preferred:
[0028] The raw material composition of the pure electrolyte includes: 75g / L copper ions, 90g / L sulfuric acid and 11mg / L chloride ions;
[0029] The additive is 3g / L collagen aqueous solution.
[0030] Preferred:
[0031] The production line speed of the foil machine is 3.7-4.1 m / min, and the winding tension is 196-270 N;
[0032] The thickness of the annular heightening member is 105-157 μm.
[0033] Further preferred:
[0034] The production line speed of the foil machine is 3.7m / min, and the winding tension is 196N;
[0035] The thickness of the annular heightening member is 105 μm.
[0036] It has been found through experiments that with the continuous optimization of the above parameters, the number of meters of stable winding can be further extended.
[0037] Compared with the prior art, the present invention has the following beneficial effects:
[0038] The present invention aims at the specific problem of the winding and folding of the raw electrolytic copper foil with high roughness of 4.5 μm or more. The production line speed and winding tension of the raw foil machine are precisely controlled during the production process. Meanwhile, the winding roller is simply improved. By winding a copper foil of a certain thickness (or other soft and windable metals, or even plastics, etc., as long as they can be used for the purpose of heightening) at both ends of the winding roller symmetrically or adding an annular gasket, the winding and folding phenomenon of the raw foil can be significantly improved. The winding length is ≥8000m, which effectively reduces the energy waste in the production process and significantly improves the yield rate. The method is simple and effective, has strong controllability, and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 It is a schematic structural diagram of a winding roller using a strip copper foil as an annular heightening member in the present invention;
[0040] Figure 2 It is a schematic structural diagram of a winding roller using an annular gasket as an annular heightening member in the present invention;
[0041] Figure 3 It is a schematic diagram of the structure of the winding roller without the annular heightening member;
[0042] In the figure, 1-winding roller, 2-annular heightening member, 3-raw foil. DETAILED DESCRIPTION
[0043] The present invention is further described in detail below in conjunction with examples and comparative examples, but the embodiments of the present invention are not limited thereto.
[0044] Unless otherwise specified, the raw materials in the examples and comparative examples of the present application were purchased through commercial channels.
[0045] Example 1
[0046] Step 1: Prepare pure electrolyte: copper ion concentration 75g / L, sulfuric acid concentration 90g / L, chloride ion concentration 11mg / L; prepare 3g / L collagen aqueous solution;
[0047] Step 2: Use two sections of 1 cm wide strip copper foil as annular heightening parts and symmetrically wind them on both ends of the winding roller, and ensure that they are in contact with both ends of the rolled raw foil, and the center line along the length direction of the copper foil is flush with the edge of the raw foil. The thickness of the wound strip copper foil is 105 μm, that is, the height of one side of the winding roller is 105 μm. Figure 1 as shown in .
[0048] Step 3: Introduce pure electrolyte and collagen aqueous solution into the electrolytic cell in the foil machine, the electrolyte temperature is 53°C, and the production current is 38KA; during the production process, the production line speed of the foil machine is controlled to be 3.7m / min and the winding tension is 196N (20kg, the winding tension can also be expressed in kg, which is calculated by dividing the tension in N by 9.8N / kg. This conversion method can be used to convert the winding tension in N to kg in Table 2 below).
[0049] The roughness of the matte surface of the raw foil prepared in this example is 4.5 μm, and the number of meters of the rolled foil is listed in Table 2 below.
[0050] Embodiment 2-3
[0051] The preparation process is basically the same as that in Example 1, except that the height of the single-side height increase, the production line speed and the winding tension are adjusted, as shown in Table 2. Table 2 also lists the winding meters of the raw foil prepared in each example.
[0052] Comparative Examples 1 to 12
[0053] The preparation process is basically the same as that in Example 1, except that the height of the single-side height increase, the production line speed, and the winding tension are adjusted, as shown in Table 2. Table 2 also lists the winding meters of the raw foil prepared in each example.
[0054] Table 2
[0055]
[0056]
[0057] The above-mentioned embodiments are preferred embodiments, but the protection scope of the present invention is not limited thereto. A person skilled in the art can easily understand the spirit of the present invention based on the above-mentioned embodiments and make different extensions and changes. However, as long as they do not deviate from the spirit of the present invention, they are all within the protection scope of the present invention.
Claims
1. A method for adjusting the rolling and folding of high-roughness electrolytic copper foil raw foil. It is characterized in that include: Prepare electrolyte to maintain stable production of raw foil, and then roll up the produced raw foil through a winding roller equipped with an annular heightening member; During the production process, the production line speed of the foil machine is controlled to be 3.7-4.4 m / min and the winding tension is controlled to be 196-343 N. There are two annular heightening members, which are symmetrically arranged at two ends of the winding roller and contact the two ends of the raw foil; The thickness of the annular heightening member is 105-210 μm.
2. The high roughness electrolytic copper foil raw foil rolling and folding adjustment method according to claim 1, It is characterized in that The roughness of the matte surface of the raw foil is ≥4.5 μm.
3. The high roughness electrolytic copper foil raw foil winding and folding adjustment method according to claim 1, It is characterized in that The width of the annular heightening member is 1 to 2 cm.
4. The method for adjusting the winding and folding of the raw electrolytic copper foil with high roughness according to claim 1, It is characterized in that The electrolyte includes a pure electrolyte and an additive; The raw material composition of the pure electrolyte includes: 20-110 g / L copper ions, 70-135 g / L sulfuric acid and 5-20 mg / L chloride ions; The additive is selected from a collagen aqueous solution with a concentration of 3 to 5 g / L.
5. The high roughness electrolytic copper foil rolling and folding adjustment method according to claim 4, Features: The raw material composition of the pure electrolyte includes: 75g / L copper ions, 90g / L sulfuric acid and 11mg / L chloride ions; The additive is 3g / L collagen aqueous solution.
6. The high roughness electrolytic copper foil rolling and folding adjustment method according to claim 1, Features: The production line speed of the foil machine is 3.7-4.1 m / min, and the winding tension is 196-270 N; The thickness of the annular heightening member is 105-157 μm.
7. The high roughness electrolytic copper foil rolling and folding adjustment method according to claim 1, Features: The production line speed of the foil machine is 3.7m / min, and the winding tension is 196N; The thickness of the annular heightening member is 105 μm.
8. A high-roughness electrolytic copper foil prepared by the adjustment method according to any one of claims 1 to 7, It is characterized in that Can stably reel ≥8000 meters.