Polyamide-6 antibacterial deodorant drawn yarn and preparation method thereof

By adding chitosan-silver/titanium dioxide composite antibacterial agent to nylon 6 fibers, blending and melting and drafting treatment, a nylon 6 antibacterial and antistatic properties was prepared, and the nanometers were solved The problem of silver hazards and antibacterial properties is not long-lasting, which improves the application range and performance of fibers.

CN119082913APending Publication Date: 2024-12-06FUJIAN KAIBANG POLYAMIDE TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411291258.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the prior art, polyamide fibers doped with nanosilver cause harm to health and the environment, their antibacterial properties are not long-lasting, and the antistatic properties of polyamide fibers are poor, affecting processing and application.

Method used

Complexes, conductive fillers, glass fibers, antioxidants, dispersants and nylon 6 slices are blended and melted with nylon 6 slices. , the nylon 6 antibacterial and anti-odorant draft wire was prepared through the screw extrusion spinning mechanism, and the drafting and winding were carried out.

Benefits of technology

It has achieved a nylon 6 antibacterial fiber with a wide antibacterial spectrum, strong antibacterial effect and long-lasting antibacterial effect. The fiber has strong antistatic properties and a wide range of application. It can be produced in conventional spinning equipment and meets the requirements of fiber physical properties.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a chinlon 6 antibacterial deodorant drawn yarn and a preparation method thereof, and relates to the field of chemical fiber processing. The preparation method comprises the following steps: (1) preparing the following components in parts by weight: 30-70 parts of chinlon 6 slices, 10-20 parts of a chitosan-silver / titanium dioxide (CA / T) composite antibacterial agent, 5-15 parts of an antistatic agent, 1-10 parts of a compound of an anionic surfactant and a nonionic surfactant, 2-10 parts of a conductive filler, 5-10 parts of glass fibers, 0.5-2 parts of an antioxidant and 2-10 parts of a dispersing agent; (2) cleaning and drying; and (3) preparing functional particles. A chitosan-silver / titanium dioxide (CA / T) composite antibacterial agent, an antistatic agent, a compound of an anionic surfactant and a nonionic surfactant, a conductive filler, glass fibers, an antioxidant and a dispersant are added into chinlon 6 for blending and melting, so that the produced chinlon antibacterial fiber has the characteristics of wide antibacterial spectrum, strong antibacterial effect, lasting antibacterial effect and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chemical fiber processing, in particular to a nylon 6 antibacterial and deodorizing drawn yarn and a preparation method thereof. Background Art

[0002] Nylon, scientific name polyamide fiber, commonly known as nylon, nylon 3 is the trade name of polyamide fiber, density 1.15g / cm, is the general name of thermoplastic resin containing repeated amide groups (-NHCO-) ​​on the main chain of the molecule. The main varieties are nylon 6 and nylon 66. Nylon silk is a fiber made of polyamide, divided into nylon filament and nylon staple. Nylon filament can be made into stretch yarn, and staple can be blended with cotton and acrylic to improve its strength and elasticity. Nylon has always occupied an important position in the clothing industry and is one of the commonly used clothing fabrics.

[0003] The Chinese invention patent with application number 201710710557.8 discloses a processing technology for long-lasting antibacterial polyester filament, which includes the following steps: a. washing and drying the thermoplastic polyurethane slices, mixing them with the antibacterial agent, adding them into a screw extruder for melting and mixing;

[0004] b. Add the cross-linking agent in the metering section of the extruder or after the extruder and before entering the mixer; c. The melt-spun material is ejected through the spinneret, spun and wound to form the finished product. The production process is: slice cleaning - drying - extrusion - mixing - spinning - drawing - cooling - oiling - winding. The antibacterial agent is silver powder, which is nano-grade silver powder.

[0005] The Chinese invention patent application number 201310088508.7 discloses a method for producing antibacterial fibers, comprising the following steps: A. Self-made antibacterial masterbatch, which comprises:

[0006] Disperse the nano silver powder in the solvent, add polypropylene slices to dissolve it after it is evenly dispersed; heat and reflux the polypropylene / nano silver system, remove the solvent in the system, dry and grind into powder; mix the polypropylene / nano silver powder and resin, extrude through a screw to prepare polypropylene antibacterial masterbatch; B, mix the antibacterial masterbatch prepared in step A with the fiber raw material at 2-10%, mix through a high-speed mixer, extrude and draw to obtain antibacterial fiber. The above technical materials all use nano silver. Although this process has an antibacterial effect, it is likely to cause the nano silver to fall off during the wearing and washing process of the made clothing, and cause harm to the human body after contact with the skin. Since the particle size of nano silver powder is small, it is easier to enter the human body. When it comes into contact with a large amount of nano silver particles, it is possible to cause harm to the liver. Studies have shown that nano silver is toxic to many aquatic organisms and can accumulate in the food chain. At the same time, the nano silver added to the fiber is easy to fall off after multiple washings, and the antibacterial performance will be greatly reduced.

[0007] At the same time, polyamide fiber is easy to pilling and generate static electricity. The surface resistance of nylon material in the existing technology is 10Ω. The charge accumulated on the surface is difficult to dissipate, which brings a lot of trouble to processing and application, affects its wearing performance, and reduces the quality of the fabric. Summary of the invention

[0008] 1. Technical issues to be resolved

[0009] In view of the shortcomings of the prior art, the present invention provides a nylon 6 antibacterial and deodorizing drawn yarn and a preparation method thereof, which solves the problems in the prior art that polyamide fibers doped with nano-silver are harmful to health and the environment, have short-lasting antibacterial properties, and have poor antistatic properties.

[0010] (II) Technical solution

[0011] To achieve the above objectives, the present invention is implemented through the following technical scheme: a method for preparing nylon 6 antibacterial and deodorizing drawn yarn, comprising:

[0012] (1) By weight: 30-70 parts of nylon 6 chips, 10-20 parts of chitosan-silver / titanium dioxide (CA / T) composite antibacterial agent, 5-15 parts of antistatic agent, 1-10 parts of a mixture of anionic surfactant and nonionic surfactant, 2-10 parts of conductive filler, 5-10 parts of glass fiber, 0.5-2 parts of antioxidant, and 2-10 parts of dispersant;

[0013] (2) Cleaning and drying: After cleaning the nylon 6 slices, use a vacuum drying oven to dry the nylon 6 slices. The drying temperature is set to 100°C, so that the moisture content of the nylon 6 slices is 110 ppm;

[0014] (3) Preparation of functional particles: Nylon 6 chips are mixed evenly with chitosan-silver / titanium dioxide (CA / T) composite antibacterial agent, antistatic agent, compound of anionic surfactant and nonionic surfactant, conductive filler, glass fiber, antioxidant, and dispersant according to a certain proportion, added into a screw extruder spinning machine, and extruded from the spinneret hole after melting to solidify into filaments;

[0015] (4) Post-processing: the prepared filaments are drawn, wound and packaged.

[0016] Preferably, in step (3), the screw temperature of the screw extruder spinning machine is 250°C-280°C, and the temperature inside the spinning box is 260°C-290°C.

[0017] Preferably, in step (4), the stretching ratio during stretching is 2-7 times, the ring blowing temperature is 10-30°C, and the ring blowing speed is 5-20 m / s.

[0018] Preferably, in step (1), the compound of the anionic surfactant and the nonionic surfactant is a compound of alkyl phosphate and polyoxyethylene ether.

[0019] Preferably, in step (1), the conductive filler is conductive zinc oxide and / or conductive tin oxide with a particle size of 10 to 100 nm.

[0020] Preferably, in step (1), the antioxidant is a phosphite antioxidant and / or a hindered phenol antioxidant.

[0021] Preferably, in step (1), the dispersant is one or at least two of polyethylene wax, polypropylene wax, EVA wax, OP wax, TAF, TAS-2A, and EBS.

[0022] The invention discloses a nylon 6 antibacterial and deodorizing drawn yarn, which is a nylon 6 antibacterial and deodorizing drawn yarn.

[0023] (III) Beneficial effects

[0024] The present invention provides a nylon 6 antibacterial and deodorizing drawn yarn and a preparation method thereof. The invention has the following beneficial effects:

[0025] By adding chitosan-silver / titanium dioxide (CA / T) composite antibacterial agent, antistatic agent, compound of anionic surfactant and nonionic surfactant, conductive filler, glass fiber, antioxidant and dispersant into nylon 6 for blending and melting, the produced nylon antibacterial fiber has the characteristics of wide antibacterial spectrum, strong antibacterial effect and lasting antibacterial effect, and the manufacturing process is simple, and it can be produced with conventional spinning equipment. The various physical properties of the fiber can meet the physical property requirements of conventional fibers, and the application range is wide. At the same time, it has strong antistatic property and lasting antistatic performance. DETAILED DESCRIPTION

[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0027] Embodiment 1:

[0028] The embodiment of the present invention provides a method for preparing nylon 6 antibacterial and deodorizing drawn yarn, comprising:

[0029] (1) By weight: 50 parts of nylon 6 chips, 15 parts of chitosan-silver / titanium dioxide (CA / T) composite antibacterial agent, 5 parts of antistatic agent, 4 parts of a mixture of anionic surfactant and nonionic surfactant, 5 parts of conductive filler, 5 parts of glass fiber, 1 part of antioxidant, and 5 parts of dispersant;

[0030] (2) Cleaning and drying: After cleaning the nylon 6 slices, use a vacuum drying oven to dry the nylon 6 slices. The drying temperature is set to 100°C, so that the moisture content of the nylon 6 slices is 110 ppm;

[0031] (3) Preparation of functional particles: Nylon 6 chips were mixed with chitosan-silver / titanium dioxide (CA / T) composite antibacterial agent, antistatic agent, compound of anionic surfactant and nonionic surfactant, conductive filler, glass fiber, antioxidant, and dispersant in proportion, added to a screw extrusion spinning machine, extruded from a spinneret after melting, and solidified into filaments. The screw temperature of the screw extrusion spinning machine was 250°C, and the temperature in the spinning box was 260°C.

[0032] (4) Post-treatment: The obtained filaments are drawn, wound and doffed. The drawing multiple during drawing is 4 times, the temperature of the annular blowing is 15° C., and the wind speed of the annular blowing is 20 m / s.

[0033] The compound of anionic surfactant and nonionic surfactant is a compound of alkyl phosphate and polyoxyethylene ether, the conductive filler is conductive zinc oxide and / or conductive tin oxide with a particle size of 70nm, the antioxidant is a phosphite antioxidant and / or a hindered phenol antioxidant, and the dispersant is one or at least two of polyethylene wax, polypropylene wax, EVA wax, OP wax, TAF, TAS-2A, and EBS.

[0034] The invention discloses a nylon 6 antibacterial and deodorizing drawn yarn, which is a nylon 6 antibacterial and deodorizing drawn yarn.

[0035] Embodiment 2:

[0036] The embodiment of the present invention provides a method for preparing nylon 6 antibacterial and deodorizing drawn yarn, comprising:

[0037] (1) By weight: 55 parts of nylon 6 chips, 16 parts of chitosan-silver / titanium dioxide (CA / T) composite antibacterial agent, 5 parts of antistatic agent, 5 parts of a mixture of anionic surfactant and nonionic surfactant, 5 parts of conductive filler, 5 parts of glass fiber, 2 parts of antioxidant, and 5 parts of dispersant;

[0038] (2) Cleaning and drying: After cleaning the nylon 6 slices, use a vacuum drying oven to dry the nylon 6 slices. The drying temperature is set to 100°C, so that the moisture content of the nylon 6 slices is 110 ppm;

[0039] (3) Preparation of functional particles: Nylon 6 chips are mixed with chitosan-silver / titanium dioxide (CA / T) composite antibacterial agent, antistatic agent, compound of anionic surfactant and nonionic surfactant, conductive filler, glass fiber, antioxidant, and dispersant in proportion, added to a screw extrusion spinning machine, extruded from a spinneret hole after melting, and solidified into filaments. The screw temperature of the screw extrusion spinning machine is 250°C-280°C, and the temperature in the spinning box is 260°C-290°C.

[0040] (4) Post-treatment: The obtained filaments are drawn, wound and doffed. The drawing multiple is 4 times, the temperature of the annular blowing is 15°C, and the wind speed of the annular blowing is 20 m / s.

[0041] The compound of anionic surfactant and nonionic surfactant is a compound of alkyl phosphate and polyoxyethylene ether, the conductive filler is conductive zinc oxide and / or conductive tin oxide with a particle size of 70nm, the antioxidant is a phosphite antioxidant and / or a hindered phenol antioxidant, and the dispersant is one or at least two of polyethylene wax, polypropylene wax, EVA wax, OP wax, TAF, TAS-2A, and EBS.

[0042] The invention discloses a nylon 6 antibacterial and deodorizing drawn yarn, which is a nylon 6 antibacterial and deodorizing drawn yarn.

[0043] Embodiment three:

[0044] The embodiment of the present invention provides a method for preparing nylon 6 antibacterial and deodorizing drawn yarn, comprising:

[0045] (1) By weight: 60 parts of nylon 6 chips, 17 parts of chitosan-silver / titanium dioxide (CA / T) composite antibacterial agent, 5 parts of antistatic agent, 5 parts of a mixture of anionic surfactant and nonionic surfactant, 5 parts of conductive filler, 5 parts of glass fiber, 1 part of antioxidant, and 2 parts of dispersant;

[0046] (2) Cleaning and drying: After cleaning the nylon 6 slices, use a vacuum drying oven to dry the nylon 6 slices. The drying temperature is set to 100°C, so that the moisture content of the nylon 6 slices is 110 ppm;

[0047] (3) Preparation of functional particles: Nylon 6 chips are mixed with chitosan-silver / titanium dioxide (CA / T) composite antibacterial agent, antistatic agent, compound of anionic surfactant and nonionic surfactant, conductive filler, glass fiber, antioxidant, and dispersant in proportion, added to a screw extrusion spinning machine, extruded from a spinneret hole after melting, and solidified into filaments. The screw temperature of the screw extrusion spinning machine is 250°C-280°C, and the temperature in the spinning box is 260°C-290°C.

[0048] (4) Post-treatment: The obtained filaments are drawn, wound and doffed. The drawing multiple during drawing is 4 times, the temperature of the annular blowing is 15° C., and the wind speed of the annular blowing is 20 m / s.

[0049] The compound of anionic surfactant and nonionic surfactant is a compound of alkyl phosphate and polyoxyethylene ether, the conductive filler is conductive zinc oxide and / or conductive tin oxide with a particle size of 70nm, the antioxidant is a phosphite antioxidant and / or a hindered phenol antioxidant, and the dispersant is one or at least two of polyethylene wax, polypropylene wax, EVA wax, OP wax, TAF, TAS-2A, and EBS.

[0050] The invention discloses a nylon 6 antibacterial and deodorizing drawn yarn, which is a nylon 6 antibacterial and deodorizing drawn yarn.

[0051] Embodiment 4:

[0052] The embodiment of the present invention provides a method for preparing nylon 6 antibacterial and deodorizing drawn yarn, comprising:

[0053] (1) By weight: 65 parts of nylon 6 chips, 18 parts of chitosan-silver / titanium dioxide (CA / T) composite antibacterial agent, 5 parts of antistatic agent, 2 parts of a mixture of anionic surfactant and nonionic surfactant, 2 parts of conductive filler, 5 parts of glass fiber, 1 part of antioxidant, and 2 parts of dispersant;

[0054] (2) Cleaning and drying: After cleaning the nylon 6 slices, use a vacuum drying oven to dry the nylon 6 slices. The drying temperature is set to 100°C, so that the moisture content of the nylon 6 slices is 110 ppm;

[0055] (3) Preparation of functional particles: Nylon 6 slices are mixed with chitosan-silver / titanium dioxide (CA / T) composite antibacterial agent, antistatic agent, compound of anionic surfactant and nonionic surfactant, conductive filler, glass fiber, antioxidant, and dispersant in proportion, added to a screw extrusion spinning machine, extruded from a spinneret hole after melting, and solidified into filaments. The screw temperature of the screw extrusion spinning machine is 250°C-280°C, and the temperature in the spinning box is 260°C-290°C.

[0056] (4) Post-treatment: The obtained filaments are drawn, wound and doffed. The drawing multiple during drawing is 4 times, the temperature of the annular blowing is 15° C., and the wind speed of the annular blowing is 20 m / s.

[0057] The compound of anionic surfactant and nonionic surfactant is a compound of alkyl phosphate and polyoxyethylene ether, the conductive filler is conductive zinc oxide and / or conductive tin oxide with a particle size of 70nm, the antioxidant is a phosphite antioxidant and / or a hindered phenol antioxidant, and the dispersant is one or at least two of polyethylene wax, polypropylene wax, EVA wax, OP wax, TAF, TAS-2A, and EBS.

[0058] The invention discloses a nylon 6 antibacterial and deodorizing drawn yarn, which is a nylon 6 antibacterial and deodorizing drawn yarn.

[0059] Embodiment five:

[0060] The embodiment of the present invention provides a method for preparing nylon 6 antibacterial and deodorizing drawn yarn, comprising:

[0061] (1) By weight: 65 parts of nylon 6 chips, 19 parts of chitosan-silver / titanium dioxide (CA / T) composite antibacterial agent, 5 parts of antistatic agent, 1 part of a mixture of anionic surfactant and nonionic surfactant, 2 parts of conductive filler, 5 parts of glass fiber, 1 part of antioxidant, and 2 parts of dispersant;

[0062] (2) Cleaning and drying: After cleaning the nylon 6 slices, use a vacuum drying oven to dry the nylon 6 slices. The drying temperature is set to 100°C, so that the moisture content of the nylon 6 slices is 110 ppm;

[0063] (3) Preparation of functional particles: Nylon 6 slices are mixed with chitosan-silver / titanium dioxide (CA / T) composite antibacterial agent, antistatic agent, compound of anionic surfactant and nonionic surfactant, conductive filler, glass fiber, antioxidant, and dispersant in proportion, added to a screw extrusion spinning machine, extruded from a spinneret hole after melting, and solidified into filaments. The screw temperature of the screw extrusion spinning machine is 250°C-280°C, and the temperature in the spinning box is 260°C-290°C.

[0064] (4) Post-treatment: The obtained filaments are drawn, wound and doffed. The drawing multiple during drawing is 4 times, the temperature of the annular blowing is 15° C., and the wind speed of the annular blowing is 20 m / s.

[0065] The compound of anionic surfactant and nonionic surfactant is a compound of alkyl phosphate and polyoxyethylene ether, the conductive filler is conductive zinc oxide and / or conductive tin oxide with a particle size of 70nm, the antioxidant is a phosphite antioxidant and / or a hindered phenol antioxidant, and the dispersant is one or at least two of polyethylene wax, polypropylene wax, EVA wax, OP wax, TAF, TAS-2A, and EBS.

[0066] The invention discloses a nylon 6 antibacterial and deodorizing drawn yarn, which is a nylon 6 antibacterial and deodorizing drawn yarn.

[0067] Embodiment six:

[0068] The embodiment of the present invention provides a method for preparing nylon 6 antibacterial and deodorizing drawn yarn, comprising:

[0069] (1) By weight: 60 parts of nylon 6 chips, 20 parts of chitosan-silver / titanium dioxide (CA / T) composite antibacterial agent, 5 parts of antistatic agent, 5 parts of a mixture of anionic surfactant and nonionic surfactant, 2 parts of conductive filler, 5 parts of glass fiber, 1 part of antioxidant, and 2 parts of dispersant;

[0070] (2) Cleaning and drying: After cleaning the nylon 6 slices, use a vacuum drying oven to dry the nylon 6 slices. The drying temperature is set to 100°C, so that the moisture content of the nylon 6 slices is 110 ppm;

[0071] (3) Preparation of functional particles: Nylon 6 chips are mixed with chitosan-silver / titanium dioxide (CA / T) composite antibacterial agent, antistatic agent, compound of anionic surfactant and nonionic surfactant, conductive filler, glass fiber, antioxidant, and dispersant in proportion, added to a screw extrusion spinning machine, extruded from a spinneret hole after melting, and solidified into filaments. The screw temperature of the screw extrusion spinning machine is 250°C-280°C, and the temperature in the spinning box is 260°C-290°C.

[0072] (4) Post-treatment: The obtained filaments are drawn, wound and doffed. The drawing multiple is 4 times, the temperature of the annular blowing is 15°C, and the wind speed of the annular blowing is 20 m / s.

[0073] The compound of anionic surfactant and nonionic surfactant is a compound of alkyl phosphate and polyoxyethylene ether, the conductive filler is conductive zinc oxide and / or conductive tin oxide with a particle size of 70nm, the antioxidant is a phosphite antioxidant and / or a hindered phenol antioxidant, and the dispersant is one or at least two of polyethylene wax, polypropylene wax, EVA wax, OP wax, TAF, TAS-2A, and EBS.

[0074] The invention discloses a nylon 6 antibacterial and deodorizing drawn yarn, which is a nylon 6 antibacterial and deodorizing drawn yarn.

[0075] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing nylon 6 antibacterial and deodorizing drawn yarn, characterized in that: include: (1) By weight: 30-70 parts of nylon 6 chips, 10-20 parts of chitosan-silver / titanium dioxide (CA / T) composite antibacterial agent, 5-15 parts of antistatic agent, 1-10 parts of a mixture of anionic surfactant and nonionic surfactant, 2-10 parts of conductive filler, 5-10 parts of glass fiber, 0.5-2 parts of antioxidant, and 2-10 parts of dispersant; (2) Cleaning and drying: After cleaning the nylon 6 slices, use a vacuum drying oven to dry the nylon 6 slices. The drying temperature is set to 100°C, so that the moisture content of the nylon 6 slices is 110 ppm; (3) Preparation of functional particles: Nylon 6 chips are mixed evenly with chitosan-silver / titanium dioxide (CA / T) composite antibacterial agent, antistatic agent, compound of anionic surfactant and nonionic surfactant, conductive filler, glass fiber, antioxidant, and dispersant according to a certain proportion, added into a screw extruder spinning machine, and extruded from the spinneret hole after melting to solidify into filaments; (4) Post-processing: the prepared filaments are drawn, wound and packaged.

2. The method for preparing the antibacterial and deodorizing drawn nylon 6 yarn according to claim 1, characterized in that: In step (3), the screw temperature of the screw extrusion spinning machine is 250°C-280°C, and the temperature inside the spinning box is 260°C-290°C.

3. The method for preparing the antibacterial and deodorizing drawn nylon 6 yarn according to claim 1, characterized in that: In step (4), the stretching ratio during stretching is 2-7 times, the ring blowing temperature is 10-30°C, and the ring blowing speed is 5-20m / s.

4. The nylon 6 antibacterial and deodorizing drawn yarn and the preparation method thereof according to claim 1, characterized in that: In step (1), the compound of the anionic surfactant and the nonionic surfactant is a compound of alkyl phosphate and polyoxyethylene ether.

5. The nylon 6 antibacterial and deodorizing drawn yarn and the preparation method thereof according to claim 1, characterized in that: In step (1), the conductive filler is conductive zinc oxide and / or conductive tin oxide with a particle size of 10 to 100 nm.

6. The antibacterial and deodorizing drawn nylon 6 yarn and the preparation method thereof according to claim 1, characterized in that: In step (1), the antioxidant is a phosphite antioxidant and / or a hindered phenol antioxidant.

7. The nylon 6 antibacterial and deodorizing drawn yarn and the preparation method thereof according to claim 1, characterized in that: In step (1), the dispersant is one or at least two of polyethylene wax, polypropylene wax, EVA wax, OP wax, TAF, TAS-2A, and EBS.

8. The antibacterial and deodorizing drawn nylon 6 yarn according to any one of claims 1 to 7, characterized in that: It is nylon 6 antibacterial and deodorizing drawn yarn.

Citation Information

Cited By

  • Durable ultraviolet-proof polyamide fiber fabric and production method thereof

    CN120889056A