Chemical method regenerated flame-retardant antibacterial low-melting cotton fiber and preparation method thereof
By copolymerizing the quaternary ammonium salt of long-chain alkylnaphthol derivative with PET waste alcoholylation product, regenerated flame retardant and antibacterial low melting point PET is solved, and the problem of insufficient flame retardant performance of fibers in the prior art is achieved and the high temperature stability of fibers is achieved Improved properties and antibacterial properties ensure that the fiber is not easy to burn at high temperatures.
Patent Information
- Application Number
- CN202411313985.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-12-06
AI Technical Summary
In the prior art, the flame retardant performance of regenerated PET fibers is insufficient, and the quaternary ammonium flame retardant decomposes at high temperatures, resulting in a decrease in flame retardant effect and difficulty in introducing into the fibers, resulting in rapid combustion of polyester fibers after long-term use.
The quaternary ammonium salt of long-chain alkylnaphthol derivative is copolymerized with PET waste alcoholylation product to form regenerated flame retardant and antibacterial low melting point PET as the cortical material of the fiber, and the copolymerized flame retardant PET is used as the core material, through copolymerization Polymerization introduces flame retardant into the fiber to improve flame retardant and antibacterial properties.
The high-temperature stability and flame retardant effect of the fiber are improved, the antibacterial properties of the fiber are enhanced, the fiber is not easy to burn at high temperatures, and the soft and fluffy properties of the fiber are improved.
Smart Images

Figure BDA0005051588530000091 
Figure BDA0005051588530000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of regenerated polyester fibers, in particular to a chemically regenerated flame-retardant, antibacterial, low-melting cotton fiber and a preparation method thereof. Background Art
[0002] Polyethylene terephthalate (PET) is an important polyester material with excellent chemical stability, electrical insulation and corrosion resistance. Therefore, PET waste is extremely difficult to degrade when left in the environment, causing serious environmental pollution. In order to solve the problem of environmental pollution caused by waste PET polyester, a technical solution for recycling and reusing waste PET polyester is proposed in the prior art. The recycling and reusing of waste PET polyester in the prior art mainly includes physical method and chemical method. The physical method is to screen and remove impurities from the waste PET polyester and then blend and granulate it into regenerated slices, such as a modification method of regenerated PET, a supercritical physical foaming shoe material and a preparation method disclosed in publication number CN117659485A. However, the quality of the regenerated slices prepared by the physical method fluctuates greatly, so they are often used as raw materials for brooms and brushes. The chemical method is to first depolymerize PET polyester into small molecules by alcoholysis, and then form regenerated PET polyester by condensation, such as a preparation method of chemically regenerated PETG polyester disclosed in publication number CN114989400B. However, the performance of PET polyester prepared by the chemical method is usually reduced, so it is usually used in the field of preparation of other low value-added short fibers.
[0003] Low melting point polyester is a new type of polyester material that has emerged in recent years. Compared with PET polyester, it has a lower melting point, which can make PET polyester soft and fluffy, and have high peel strength. It is often used as a skin layer polyester material in combination with core layer PET polyester, so that cotton fiber has a soft and fluffy feel and the elastic properties of PET polyester. Since the skin layer PET polyester mainly provides the characteristics of softness and fluffiness, the chemically regenerated PET polyester can be used as a raw material for low melting point polyester to prepare recycled low melting point PET polyester.
[0004] Polyester materials are flammable. Therefore, in order to improve the flame retardant properties of polyester fibers, flame retardants are added to polyester fibers in the prior art to improve the flame retardant properties of polyester fibers. Currently disclosed polyester fiber flame retardants include halogen flame retardants, phosphorus flame retardants, nitrogen flame retardants and inorganic flame retardants, among which nitrogen flame retardants are mainly quaternary ammonium salt flame retardants. Currently commonly used quaternary ammonium salt flame retardants will decompose into ammonia and nitric acid at 110°C, so they are often used as finishing agents on the surface of fibers. However, the finishing agents are only attached to the surface of the fibers and will be separated from the fiber surface during long-term use, resulting in a decrease in the flame retardant effect. In addition, quaternary ammonium salt flame retardants achieve flame retardant effects through rapid endothermic reactions. Therefore, when used as finishing agents, they can only exert flame retardant effects on polyester fibers for a short time. When the finishing agent on the surface of the polyester fiber is completely ineffective, the polyester inside the polyester fiber will still burn rapidly. Therefore, it is of great significance to provide a quaternary ammonium salt flame retardant that can be introduced into the polyester fiber. Summary of the invention
[0005] In order to overcome the problem that the recycled PET in the prior art can only be applied in low value-added fields, the present invention provides a chemically recycled flame-retardant, antibacterial and low-melting cotton fiber and a preparation method thereof. The fiber material is a skin-core structure, the skin layer is recycled flame-retardant, antibacterial and low-melting-point PET, and the core layer is copolymerized flame-retardant PET. The recycled flame-retardant, antibacterial and low-melting-point PET in the skin layer is a low-melting-point PET copolymerized by using a long-chain alkylnaphthol derivative quaternary ammonium salt and a PET waste alcoholysis product. The long-chain alkylnaphthol derivative quaternary ammonium salt will not decompose in the PET polymerization reaction. At the same time, the long-chain alkyl structure contained in the long-chain alkylnaphthol derivative quaternary ammonium salt can also reduce the melting point of PET. In addition, the alkylnaphthol derivative quaternary ammonium salt also has excellent antibacterial properties, so that the prepared recycled flame-retardant, antibacterial and low-melting-point PET has the advantages of antibacterial, flame retardant, soft and fluffy.
[0006] The specific technical scheme of the present invention is: The invention discloses a chemically regenerated flame-retardant, antibacterial, low-melting cotton fiber. The cotton fiber is a skin-core structure. The raw material of the core layer of the skin-core structure is copolymerized flame-retardant PET. The raw material of the skin layer of the skin-core structure is regenerated flame-retardant, antibacterial, low-melting-point PET. The regenerated flame-retardant, antibacterial, low-melting-point PET is copolymerized with quaternary ammonium salt and alcoholysis product of PET waste as raw materials.
[0007] Preferably, the quaternary ammonium salt is a quaternary ammonium salt of a long-chain alkyl naphthol derivative.
[0008] Preferably, the quaternary ammonium salt is prepared by reacting chloroacetyl organic amine and a long-chain alkyl naphthol derivative.
[0009] Preferably, the chloroacetyl organic amine is one of chloroacetyl decylamine, chloroacetyl dodecylamine and chloroacetyl tetradecylamine.
[0010] Preferably, the long-chain alkylnaphthol derivative is prepared by alkylation reaction of organic amine and long-chain olefin.
[0011] Preferably, the organic amine is N-acetyl-(1-naphthyloxy)-N,N-dimethylethylenediamine.
[0012] Preferably, the long-chain olefin is a C12 olefin.
[0013] Preferably, the alcoholysis product of the PET waste includes one or more of regenerated terephthalic acid, regenerated dimethyl terephthalate, regenerated ethylene terephthalate and ethylene glycol.
[0014] The invention provides a chemically regenerated flame-retardant and antibacterial low-melting cotton fiber, wherein the cortex is regenerated flame-retardant and antibacterial low-melting-point PET, and the core layer is copolymerized flame-retardant PET. The polyester raw materials for the cortex and core layers of the cotton fiber of the invention both adopt copolymerized flame-retardant polyester, and the copolymerized flame-retardant polyester is prepared by copolymerization by adding a flame retardant in the polyester copolymerization synthesis stage. The advantage of using the copolymerized flame-retardant polyester is that the problem of changing the performance of the polyester fiber by blending the flame retardant with the polyester and treating the polyester surface with a flame retardant finishing agent can be avoided. In addition, adding the flame retardant in the copolymerization stage of the polyester fiber can introduce the flame retardant between the polyester molecules, and the flame retardant effect is better than blending and surface treatment.
[0015] The cortical material of the invention is a regenerated antibacterial low-melting polyester. The regenerated antibacterial low-melting polyester is synthesized by copolymerizing a PET waste alcoholysis product obtained by chemically depolymerizing PET waste with a long-chain alkyl naphthol derivative quaternary ammonium salt as a raw material. The long-chain alkyl naphthol derivative quaternary ammonium salt is a high-temperature resistant quaternary ammonium salt prepared by reacting a long-chain alkyl naphthol derivative with a quaternary ammonium salt. The long-chain alkyl naphthol derivative quaternary ammonium salt will not decompose in the entire reaction system of PET synthesis, and the quaternary ammonium salt can be introduced into PET molecules. The long-chain alkyl naphthol quaternary ammonium salt also contains a long-chain alkyl branched chain. The long-chain alkyl branched chain can reduce the melting point of the PET polyester in the PET copolymerization stage, so that the low-melting point PET polyester has soft and fluffy performance as a cortical structure. In addition, the long-chain alkyl naphthol derivative quaternary ammonium salt also has excellent antibacterial function, and can give the cortical PET polyester excellent antibacterial performance.
[0016] A method for preparing the above-mentioned chemically regenerated flame-retardant and antibacterial low-melting cotton fiber comprises the following steps: Step 1: performing an alkylation reaction on an organic amine and a long-chain olefin under the action of a catalyst to prepare a long-chain alkyl naphthol derivative, and adding the long-chain alkyl naphthol derivative and a chloroacetyl organic amine into a solvent for reaction to prepare a quaternary ammonium salt of the long-chain alkyl naphthol derivative; Step 2: Screening and crushing the PET polyester waste to obtain PET waste fragments, heating the PET waste fragments until they are melted, adding diol and a catalyst to perform primary alcoholysis and secondary alcoholysis respectively to obtain PET waste alcoholysis products, and uniformly mixing the PET alcoholysis products and a quaternary ammonium salt of a long-chain alkyl naphthol derivative to perform esterification reaction and polycondensation reaction to prepare a regenerated flame-retardant, antibacterial, low-melting-point PET; Step 3: adding 1,2-dicarboxyethyldiphenylphosphine oxide, terephthalic acid, ethylene glycol, a catalyst and a stabilizer into a container to respectively carry out esterification reaction and polycondensation reaction to prepare copolymer flame-retardant PET; Step 4: After drying, the copolymerized flame-retardant PET and the regenerated flame-retardant antibacterial low-melting-point PET are injected into a melt spinning device for skin-core composite spinning to produce chemically regenerated flame-retardant antibacterial low-melting cotton fibers.
[0017] Preferably, the catalyst is one of HY molecular sieve and Hβ molecular sieve.
[0018] Preferably, the preparation method according to claim 1 is characterized in that the conditions of the alkylation reaction in step 1 include: reaction temperature 130-160° C., reaction pressure 0.5-2 MPa.
[0019] Preferably, in step 1, the molar ratio of N-acetyl-(1-naphthyloxy)-N,N-dimethylethylenediamine to C12 olefin is 3 to 6:1.
[0020] Preferably, the diol in step 2 is one or more of ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butylene glycol, 1,4-butylene glycol, 1,5-pentanediol, 2,2-dimethyl-1,3-propylene glycol, 2-ethyl-2-tert-butyl-1,3-propylene glycol or 2,2,4-trimethyl-1,6-hexanediol.
[0021] Preferably, the catalyst in step 2 is zinc acetate, and the amount of zinc acetate used is 0.5-1.5 wt%.
[0022] Compared with the prior art, this application has the following technical effects: The invention provides a flame-retardant, antibacterial, low-melting cotton fiber and a preparation method thereof. The fiber material is a skin-core structure, the skin layer is a regenerated antibacterial, flame-retardant, and low-melting-point PET, the core layer is a copolymerized flame-retardant PET, and the skin layer is regenerated flame-retardant, antibacterial, and low-melting-point PET is copolymerized by using a long-chain alkylnaphthol derivative quaternary ammonium salt and a PET waste alcoholysis product. The long-chain alkylnaphthol derivative quaternary ammonium salt will not be decomposed in the PET polymerization reaction. At the same time, the long-chain alkyl structure contained in the long-chain alkylnaphthol derivative quaternary ammonium salt can also reduce the melting point of PET. In addition, the long-chain alkylnaphthol derivative quaternary ammonium salt also has excellent antibacterial performance, and can make the prepared regenerated flame-retardant, antibacterial, and low-melting-point PET have the advantages of antibacterial, flame retardant, softness, and fluffiness. DETAILED DESCRIPTION
[0023] The present invention will be further described below in conjunction with the embodiments.
[0024] Embodiment 1: The invention discloses a chemically regenerated flame-retardant, antibacterial and low-melting cotton fiber. The cotton fiber has a skin-core structure. The raw material of the cotton fiber core layer is copolymerized flame-retardant PET, and the raw material of the cotton fiber skin layer is recycled flame-retardant, antibacterial and low-melting-point PET.
[0025] A method for preparing the above-mentioned chemically regenerated flame-retardant and antibacterial low-melting cotton fiber comprises the following steps: Step 1: N-acetyl-(1-naphthyloxy)-N,N-dimethylethylenediamine, C12 olefin and solvent (cyclohexane) in a molar ratio of 6:1:60 are mixed evenly and transported to a reaction vessel through a quantitative pump for alkylation reaction to obtain a crude product. The alkylation reaction conditions are: reaction temperature 160°C, reaction pressure 1MPa, reaction time 6h, HY molecular sieve (particle size 20-40 mesh) is provided in the reaction vessel, and the crude product is filtered and then precipitated with acetone / isoamyl alcohol (mass ratio 1:3 ) mixed solvent for crystallization separation to obtain long-chain alkyl naphthol derivatives; adding the long-chain alkyl naphthol derivatives and chloroacetyldecylamine to a methanol / ethanol mixture with a volume ratio of 1:1, stirring at a temperature of 120°C for 32 hours to obtain a crude product, the crude product is rotary evaporated in a 60°C water bath at a speed of 110r / min to obtain a purified product, and then the purified product is added to an ethanol / petroleum ether mixture (volume ratio of 1:4) solvent for recrystallization to obtain a quaternary ammonium salt of a long-chain alkyl naphthol derivative.
[0026] Step 2: Screening and crushing the PET polyester waste to obtain PET waste fragments, heating 100 g of the PET waste fragments at 260-270° C. under a nitrogen atmosphere until melted, then adding 160 g of cyclopentanediol and 0.5 g of zinc acetate, stirring and continuously passing nitrogen, performing primary alcoholysis for 5 min under the action of 500 W microwaves, filtering the primary alcoholysis product through a 3000 μm filter and a 300 μm filter to obtain a primary alcoholysis product, adding 90 g of cyclopentanediol and 0.2 g of zinc acetate to 60 g of the primary alcoholysis product, stirring and continuously passing nitrogen, and performing secondary alcoholysis for 5 min under the action of 400 W microwaves. min, the secondary alcoholysis product was decolorized by activated carbon and filtered through a 300 μm filter to obtain the alcoholysis product of PET waste, 40 g of the alcoholysis product of PET waste, 120 g of terephthalic acid, ethylene glycol and quaternary ammonium salt of long-chain alkylnaphthol derivative (the mass ratio of terephthalic acid and ethylene glycol was 1:1.56:0.05) were mixed evenly and then subjected to esterification reaction at a temperature of 250-260°C. After the esterification reaction was completed, 0.02% of catalyst (butyl phthalate) and 0.03% of stabilizer (trimethyl phosphate) were added and the reaction was maintained at 260-280°C for 2h for polycondensation reaction to prepare recycled flame-retardant, antibacterial and low-melting-point PET.
[0027] Step 3: Mix terephthalic acid, ethylene glycol and 2-dicarboxyethyldiphenylphosphine oxide in a molar ratio of 1:1.5:0.05 and inject them into a reactor, introduce nitrogen and heat to 250-260°C for esterification reaction. After the esterification reaction is completed, add 0.02% of catalyst (butyl phthalate) and 0.03% of stabilizer (trimethyl phosphate) and react for 30 minutes at a pressure of 500Pa and a temperature of 260°C, and then react for 50 minutes at a pressure of 100Pa and a temperature of 25°C to prepare a copolymer flame-retardant PET.
[0028] Step 4: Dry the recycled flame retardant antibacterial low melting point PET and copolymer flame retardant PET in an oven at 80°C for 24 hours, and then inject the dried recycled flame retardant antibacterial low melting point PET and copolymer flame retardant PET slices into the spinning device respectively. The temperature sections of the cortical screw are: Zone 1 200-260°C, Zone 2 200-260°C, Zone 3 200-260°C, Zone 4 200-260°C, Zone 5 200-260°C, Zone 6 200-260°C, Zone 7 200-260°C, Zone 8 200-260°C, Zone 9 200-260°C, Zone 10 200-260°C The temperature sections of the core layer screw are: zone 1 250-280°C, zone 2 250-280°C, zone 3 250-280°C, zone 4 250-280°C, zone 5 250-280°C. After extrusion, the screw enters the spinning box and is extruded through the spinning assembly and subjected to ring blowing (ring blowing temperature 20°C, ring blowing speed 5m / s) to form sheath-core composite fiber filaments. The sheath-core composite fiber filaments are cold-drawn into pre-spinning, and the pre-spinning stretching ratio is 100-400%. The pre-spinning is then placed in a post-spinning device for stretching to form chemically regenerated flame-retardant, antibacterial, and low-melting cotton fibers, with a total stretching ratio of 200%.
[0029] Embodiment 2: The invention discloses a chemically regenerated flame-retardant, antibacterial and low-melting cotton fiber. The cotton fiber has a skin-core structure. The raw material of the cotton fiber core layer is copolymerized flame-retardant PET, and the raw material of the cotton fiber skin layer is recycled flame-retardant, antibacterial and low-melting-point PET.
[0030] A method for preparing the above-mentioned chemically regenerated flame-retardant and antibacterial low-melting cotton fiber comprises the following steps: Step 1: N-acetyl-(1-naphthyloxy)-N,N-dimethylethylenediamine, C12 olefin and solvent (cyclohexane) in a molar ratio of 4:1:60 are mixed evenly and transported to a reaction vessel through a quantitative pump for alkylation reaction to obtain a crude product. The alkylation reaction conditions are: reaction temperature 150°C, reaction pressure 2MPa, reaction time 12h, HY molecular sieve (particle size 20-40 mesh) is provided in the reaction vessel, and the crude product is filtered and then precipitated with acetone / isoamyl alcohol (mass ratio 1: 4) using a mixed solvent for crystallization separation to obtain a long-chain alkyl naphthol derivative; adding the long-chain alkyl naphthol derivative and chloroacetyldecylamine to a methanol / ethanol mixture in a volume ratio of 1:1, stirring at 120°C for 32 hours to obtain a crude product, and rotary evaporating the crude product in a 60°C water bath at a speed of 110 r / min to obtain a purified product, and then adding the purified product to an ethanol / petroleum ether mixture (volume ratio of 1:4) for recrystallization to obtain a quaternary ammonium salt of a long-chain alkyl naphthol derivative.
[0031] Step 2: Screening and crushing the PET polyester waste to obtain PET waste fragments, heating 100 g of the PET waste fragments at 260-270° C. under a nitrogen atmosphere until melted, then adding 160 g of cyclopentanediol and 0.5 g of zinc acetate, stirring and continuously passing nitrogen, performing primary alcoholysis for 5 min under the action of 500 W microwaves, filtering the primary alcoholysis product through a 3000 μm filter and a 300 μm filter to obtain a primary alcoholysis product, adding 90 g of cyclopentanediol and 0.2 g of zinc acetate to 60 g of the primary alcoholysis product, stirring and continuously passing nitrogen, and performing secondary alcoholysis for 5 min under the action of 400 W microwaves. min, the secondary alcoholysis product was decolorized by activated carbon and filtered through a 300 μm filter to obtain the alcoholysis product of PET waste, 40 g of the alcoholysis product of PET waste, 120 g of terephthalic acid, ethylene glycol and quaternary ammonium salt of long-chain alkylnaphthol derivative (the mass ratio of terephthalic acid and ethylene glycol was 1:1.56:0.05) were mixed evenly and then subjected to esterification reaction at a temperature of 250-260°C. After the esterification reaction was completed, 0.02% of catalyst (butyl phthalate) and 0.03% of stabilizer (trimethyl phosphate) were added and the reaction was maintained at 260-280°C for 2h for polycondensation reaction to prepare recycled flame-retardant, antibacterial and low-melting-point PET.
[0032] Step 3: 1, ethylene glycol and 2-dicarboxyethyldiphenylphosphine oxide in a molar ratio of 1:1.5:0.05 are mixed evenly and injected into a reactor, nitrogen is introduced and the temperature is raised to 230°C for esterification reaction, and the esterification rate is maintained above 96%. After the esterification reaction is completed, 0.02% of a catalyst (butyl phthalate) and 0.03% of a stabilizer (trimethyl phosphate) are added for polycondensation reaction. The polycondensation reaction is first reacted at a pressure of 500 Pa and a temperature of 260°C for 30 minutes, and then reacted at a pressure of 100 Pa and a temperature of 25°C for 50 minutes to prepare a copolymer flame-retardant PET.
[0033] Step 4: Dry the recycled flame retardant antibacterial low melting point PET and copolymer flame retardant PET in an oven at 80°C for 24 hours, and then inject the dried recycled flame retardant antibacterial low melting point PET and copolymer flame retardant PET into the spinning device respectively. The temperature sections of the cortical screw are: zone 1 200-260°C, zone 2 200-260°C, zone 3 200-260°C, zone 4 200-260°C, zone 5 200-260°C, zone 6 200-260°C, zone 7 200-260°C, zone 8 200-260°C, zone 9 200-260°C, zone 10 200-260°C The core layer screw temperature sections are: zone 1 250-280°C, zone 2 250-280°C, zone 3 250-280°C, zone 4 250-280°C, zone 5 250-280°C. After extrusion, the screw enters the spinning box and is extruded through the spinning assembly and subjected to ring blowing (ring blowing temperature 10°C, ring blowing speed 0.5m / s) to form sheath-core composite fiber filaments. The sheath-core composite fiber filaments are cold-drawn into front spinning with a front spinning stretching ratio of 100%. The front spinning is then placed in a post-spinning device for stretching to form chemically regenerated flame-retardant, antibacterial, and low-melting cotton fibers with a total stretching ratio of 400%.
[0034] Embodiment 3: The invention discloses a chemically regenerated flame-retardant, antibacterial and low-melting cotton fiber. The cotton fiber has a skin-core structure. The raw material of the cotton fiber core layer is copolymerized flame-retardant PET, and the raw material of the cotton fiber skin layer is recycled flame-retardant, antibacterial and low-melting-point PET.
[0035] A method for preparing the above-mentioned chemically regenerated flame-retardant and antibacterial low-melting cotton fiber comprises the following steps: Step 1: N-acetyl-(1-naphthyloxy)-N, N-dimethylethylenediamine, C12 olefin and solvent (cyclohexane) in a molar ratio of 3:1:60 are mixed evenly and transported to a reaction vessel through a quantitative pump for alkylation reaction to obtain a crude product. The alkylation reaction conditions are: reaction temperature 160°C, reaction pressure 0.5MPa, reaction time 24h, and Hβ molecular sieve (particle size 40-80 mesh) is provided in the reaction vessel. The crude product is filtered and then precipitated with acetone / isoamyl alcohol (mass ratio 1 :3) using a mixed solvent for crystallization separation to obtain a long-chain alkyl naphthol derivative; adding the long-chain alkyl naphthol derivative and chloroacetyldecylamine to a methanol / ethanol mixture in a volume ratio of 1:1, stirring at 120°C for 32 hours to prepare a crude product, and rotary evaporating the crude product in a 60°C water bath at a speed of 110 r / min to obtain a purified product, and then adding the purified product to an ethanol / petroleum ether mixture (volume ratio of 1:4) solvent for recrystallization to obtain a quaternary ammonium salt of a long-chain alkyl naphthol derivative.
[0036] Step 2: Screening and crushing the PET polyester waste to obtain PET waste fragments, heating 100 g of the PET waste fragments at 260-270° C. under a nitrogen atmosphere until melted, then adding 160 g of cyclopentanediol and 0.5 g of zinc acetate, stirring and continuously passing nitrogen, performing primary alcoholysis for 5 min under the action of 500 W microwaves, filtering the primary alcoholysis product through a 3000 μm filter and a 300 μm filter to obtain a primary alcoholysis product, adding 90 g of cyclopentanediol and 0.2 g of zinc acetate to 60 g of the primary alcoholysis product, stirring and continuously passing nitrogen, and performing secondary alcoholysis for 5 min under the action of 400 W microwaves. min, the secondary alcoholysis product was decolorized by activated carbon and filtered through a 300 μm filter to obtain the alcoholysis product of PET waste, 40 g of the alcoholysis product of PET waste, 120 g of terephthalic acid, ethylene glycol and quaternary ammonium salt of long-chain alkylnaphthol derivative (the mass ratio of terephthalic acid and ethylene glycol was 1:1.56:0.05) were mixed evenly and then subjected to esterification reaction at a temperature of 250-260°C. After the esterification reaction was completed, 0.02% of catalyst (butyl phthalate) and 0.03% of stabilizer (trimethyl phosphate) were added and the reaction was maintained at 260-280°C for 2h for polycondensation reaction to prepare recycled flame-retardant, antibacterial and low-melting-point PET.
[0037] Step 3: 1, ethylene glycol and 2-dicarboxyethyldiphenylphosphine oxide in a molar ratio of 1:1.5:0.05 are mixed evenly and injected into a reactor, nitrogen is introduced and the temperature is raised to 230°C for esterification reaction, and the esterification rate is maintained above 96%. After the esterification reaction is completed, 0.02% of a catalyst (butyl phthalate) and 0.03% of a stabilizer (trimethyl phosphate) are added for polycondensation reaction. The polycondensation reaction is first reacted at a pressure of 500 Pa and a temperature of 260°C for 30 minutes, and then reacted at a pressure of 100 Pa and a temperature of 25°C for 50 minutes to prepare a copolymer flame-retardant PET.
[0038] Step 4: Dry the recycled flame retardant antibacterial low melting point PET and copolymer flame retardant PET in an oven at 80°C for 24 hours, and then inject the dried recycled flame retardant antibacterial low melting point PET and copolymer flame retardant PET into the spinning device respectively. The temperature sections of the cortical screw are: zone 1 200-260°C, zone 2 200-260°C, zone 3 200-260°C, zone 4 200-260°C, zone 5 200-260°C, zone 6 200-260°C, zone 7 200-260°C, zone 8 200-260°C, zone 9 200-260°C, zone 10 200-260°C The temperature sections of the core layer screw are: zone 1 250-280°C, zone 2 250-280°C, zone 3 250-280°C, zone 4 250-280°C, zone 5 250-280°C. After extrusion, the screw enters the spinning box and is extruded through the spinning assembly and subjected to ring blowing (ring blowing temperature 30°C, ring blowing speed 10m / s) to form sheath-core composite fiber filaments. The sheath-core composite fiber filaments are cold-drawn into front spinning with a front spinning stretching ratio of 200%. The front spinning is then placed in a post-spinning device for stretching to form chemically regenerated flame-retardant, antibacterial, and low-melting cotton fibers with a total stretching ratio of 200%.
[0039] Embodiment 4: The invention discloses a chemically regenerated flame-retardant, antibacterial and low-melting cotton fiber. The cotton fiber has a skin-core structure. The raw material of the cotton fiber core layer is copolymerized flame-retardant PET, and the raw material of the cotton fiber skin layer is recycled flame-retardant, antibacterial and low-melting-point PET.
[0040] A method for preparing the above-mentioned chemically regenerated flame-retardant and antibacterial low-melting cotton fiber comprises the following steps: Step 1: N-acetyl-(1-naphthyloxy)-N, N-dimethylethylenediamine, C12 olefin and solvent (cyclohexane) in a molar ratio of 6:1:60 are mixed evenly and transported to a reaction vessel through a quantitative pump for alkylation reaction to obtain a crude product. The alkylation reaction conditions are: reaction temperature 130-160°C, reaction pressure 0.5-2MPa, reaction time 12h, HY molecular sieve (particle size 20-40 mesh) is provided in the reaction vessel, and the crude product is filtered and then precipitated with acetone / isoamyl alcohol (mass ratio The long-chain alkyl naphthol derivatives were separated by crystallization in a mixed solvent of ethanol / trichloromethane (volume ratio 1:3); the long-chain alkyl naphthol derivatives and chloroacetyltetradecylamine were added to a mixed solution of acetonitrile / n-pentane (volume ratio 1:2), stirred at 100°C for 40 hours to prepare a crude product, the crude product was rotary evaporated in a water bath at 80°C and a speed of 120 r / min to obtain a purified product, and the purified product was added to an ethanol / trichloromethane mixed solution (volume ratio 1:3) solvent for recrystallization to obtain a quaternary ammonium salt of a long-chain alkyl naphthol derivative.
[0041] Step 2: Screening and crushing the PET polyester waste to obtain PET waste fragments, heating 100 g of the PET waste fragments at 260-270° C. under a nitrogen atmosphere until melted, then adding 160 g of cyclopentanediol and 0.5 g of zinc acetate, stirring and continuously passing nitrogen, performing primary alcoholysis for 5 min under the action of 500 W microwaves, filtering the primary alcoholysis product through a 3000 μm filter and a 300 μm filter to obtain a primary alcoholysis product, adding 90 g of cyclopentanediol and 0.2 g of zinc acetate to 60 g of the primary alcoholysis product, stirring and continuously passing nitrogen, and performing secondary alcoholysis for 5 min under the action of 400 W microwaves. min, the secondary alcoholysis product was decolorized by activated carbon and filtered through a 300 μm filter to obtain the alcoholysis product of PET waste, 40 g of the alcoholysis product of PET waste, 120 g of terephthalic acid, ethylene glycol and quaternary ammonium salt of long-chain alkylnaphthol derivative (the mass ratio of terephthalic acid and ethylene glycol was 1:1.56:0.05) were mixed evenly and then subjected to esterification reaction at a temperature of 250-260°C. After the esterification reaction was completed, 0.02% of catalyst (butyl phthalate) and 0.03% of stabilizer (trimethyl phosphate) were added and the reaction was maintained at 260-280°C for 2h for polycondensation reaction to prepare recycled flame-retardant, antibacterial and low-melting-point PET.
[0042] Step 3: 1, ethylene glycol and 2-dicarboxyethyldiphenylphosphine oxide in a molar ratio of 1:1.5:0.05 are mixed evenly and injected into a reactor, nitrogen is introduced and the temperature is raised to 230°C for esterification reaction, and the esterification rate is maintained above 96%. After the esterification reaction is completed, 0.02% of a catalyst (butyl phthalate) and 0.03% of a stabilizer (trimethyl phosphate) are added for polycondensation reaction. The polycondensation reaction is first reacted at a pressure of 500 Pa and a temperature of 260°C for 30 minutes, and then reacted at a pressure of 100 Pa and a temperature of 25°C for 50 minutes to prepare a copolymer flame-retardant PET.
[0043] Step 4: Dry the recycled flame retardant antibacterial low melting point PET and copolymer flame retardant PET in an oven at 80°C for 24 hours, and then inject the dried recycled flame retardant antibacterial low melting point PET and copolymer flame retardant PET into the spinning device respectively. The temperature sections of the cortical screw are: zone 1 200-260°C, zone 2 200-260°C, zone 3 200-260°C, zone 4 200-260°C, zone 5 200-260°C, zone 6 200-260°C, zone 7 200-260°C, zone 8 200-260°C, zone 9 200-260°C, zone 10 200-260°C. ℃; the core layer screw temperature sections are: zone 1 250-280℃, zone 2 250-280℃, zone 3 250-280℃, zone 4 250-280℃, zone 5 250-280℃. After extrusion, the screw enters the spinning box and then is extruded through the spinning assembly and subjected to ring blowing (ring blowing temperature 20℃, ring blowing speed 5m / s) to form sheath-core composite fiber filaments. The sheath-core composite fiber filaments are cold-drawn into front-spinning, and the front-spinning stretching ratio is 200%. The front-spinning is then placed in a post-spinning device for drawing to form chemically regenerated flame-retardant, antibacterial, and low-melting cotton fibers, with a total drawing ratio of 200%.
[0044] Comparative Example 1: Compared with Example 1, in Comparative Example 1, ordinary low-melting point PET is used as the sheath polyester material and copolymerized flame-retardant PET to make a flame-retardant low-melting point cotton fiber with a sheath-core structure, and then a quaternary ammonium salt flame retardant finishing agent is used to surface treat the fiber sheath.
[0045] Comparative Example 2: Compared with Example 1, the recycled flame retardant and antibacterial PET made of quaternary ammonium salt of long-chain alkyl naphthol derivatives in Example 1 is blended with ordinary low-melting point PET polyester to obtain a blended recycled flame retardant and antibacterial low-melting point PET, and then the blended recycled flame retardant and antibacterial low-melting point PET is used as the skin layer and the copolymerized flame retardant PET is used as the core layer to prepare a chemically recycled flame retardant and antibacterial low-melting point cotton fiber with a skin-core structure.
[0046] Comparative Example 3: Compared with Example 4, in Comparative Example 3, ordinary low-melting-point PET is used as the sheath polyester material and copolymerized flame-retardant PET to make a flame-retardant low-melting-point cotton fiber with a sheath-core structure, and then a quaternary ammonium salt flame retardant finishing agent is used to surface treat the fiber sheath.
[0047] Comparative Example 4: Compared with Example 4, the recycled flame retardant and antibacterial PET made of quaternary ammonium salt of long-chain alkyl naphthol derivatives in Example 4 is blended with ordinary low-melting point PET polyester to obtain blended recycled flame retardant and antibacterial low-melting point PET, and then the blended recycled flame retardant and antibacterial low-melting point PET is used as the skin layer polyester and the copolymerized flame retardant PET is used as the core layer to prepare a chemically recycled flame retardant and antibacterial low-melting point cotton fiber with a skin-core structure.
[0048] Test example: The antibacterial properties, flame retardant properties, fabric surface properties and physical and chemical properties of the chemically regenerated flame retardant and antibacterial low-melting cotton fibers obtained in Examples 1 to 5 and Comparative Examples 1 to 6 were tested; The physical and chemical properties test methods refer to GB / T 14344-2022 Test method for tensile properties of chemical fiber filaments and FZ / T50004-2011 Test method for dry heat shrinkage of polyester staple fibers; The antibacterial performance test method refers to "GB / T 20944-2007 Evaluation of Antibacterial Performance of Textiles"; The flame retardant performance test method refers to GB / T 5454: Determination of the burning performance of textiles by oxygen index method; Fabric surface performance test The KES-FB instrument was used to test the average friction coefficient and surface roughness of the fabric; The physical and chemical properties test performance is shown in Table 1; The test results of flame retardancy, antibacterial properties and fabric surface properties are shown in Table 2; Table 1 Physical and chemical properties test results Breaking strength (cN / dtex) Elongation at break (%) 125℃ dry heat shrinkage (%) Example 1 1.54 178 14 Example 2 1.62 162 13 Example 3 1.83 173 14 Example 4 2.33 152 11 Table 2 Flame retardant and antibacterial properties test results As shown in Table 1, the physical and chemical properties of the chemically regenerated flame retardant and antibacterial low-melting cotton fibers prepared in Examples 1 to 4 show that the flame retardant and antibacterial low-melting cotton fibers prepared by the present invention have a breaking strength between 1.5 and 4.0 cN / dtex, an elongation at break between 40 and 180%, and a dry heat shrinkage at 125°C of less than 15%, and have excellent fiber strength and elastic properties.
[0049] As shown in Table 2, the chemically regenerated flame-retardant and antibacterial low-melting cotton fibers prepared in Examples 1 to 4 have an antibacterial property of more than 99% against Candida albicans, Escherichia coli and Staphylococcus aureus, and a limiting oxygen index greater than 30%, which makes them flame-retardant materials with excellent flame retardant effects.
[0050] In Comparative Examples 1 to 4, the flame retardant finishing agent and the flame retardant blending were tested respectively. After analyzing the test results, it was found that the antibacterial properties of the fiber after using the flame retardant finishing agent against Candida albicans, Escherichia coli and Staphylococcus aureus all reached more than 99%, but the antibacterial effect of the blended cotton fiber on Candida albicans, Escherichia coli and Staphylococcus aureus was only more than 90%. The above results show that the long-chain alkyl naphthol derivative quaternary ammonium salt prepared in the present application has excellent antibacterial properties, and the finishing agent and copolymerization synthesis can make the antibacterial effect of the long-chain alkyl naphthol derivative quaternary ammonium salt more significant. In order to ensure the mechanical properties of the blended fiber, the blending ratio needs to be controlled, resulting in the antibacterial effect of the long-chain alkyl naphthol derivative quaternary ammonium salt being limited and unable to fully exert its antibacterial properties.
[0051] After analyzing the flame retardant performance results of Comparative Examples 1 to 4 and Examples 1 to 4, it was found that the oxygen limit index of the flame retardant cotton fibers obtained in Examples 1 to 4, Comparative Example 2, and Comparative Example 4 was above 27%, and they all belonged to flame retardant materials. However, the oxygen limit index of Comparative Example 2 and Comparative Example 4 was less than that of Examples 1 to 4, and the oxygen limit index of the flame retardant cotton fibers of Example 1, Comparative Example 1, and Comparative Example 3 was less than 22%, and they belonged to flammable materials. The above results show that the flame retardant performance of the regenerated flame retardant antibacterial cotton fiber provided by the present application is more significant. In addition, it was found in the experiment that since the cortex of the present application adopts low melting point polyester, the flame burning will easily cause the cortex polyester to melt and drip. Since the polyester cotton fiber using the flame retardant finishing agent in Example 1 and Comparative Example 3 can only perform flame retardant treatment on the polyester surface, the low-melting point polyester in the cortical polyester that has not been treated with the finishing agent will burn rapidly after dripping; in addition, although the blended quaternary ammonium salt flame retardant will form a foam covering layer, since the ratio of the flame retardant polyester to the ordinary polyester needs to be strictly controlled during the blending process, the problem of incomplete coverage of the flame retardant foam covering layer will occur, and the uncovered part will still burn when continuously exposed to the fire source, while the copolymerized polyester fiber provided in the present application will form a uniform foam covering layer on the cortex after contacting the source, protecting the low-melting point polyester from dripping and thus avoiding fiber burning.
[0052] The feel of plant fibers is usually related to the friction performance and roughness of the fabric surface. From the average friction coefficient and surface roughness results in Table 2, it can be seen that when ordinary PET is used as the surface layer in Comparative Examples 1 and 3, the roughness of the fabric surface is higher than that in Examples 1 to 4. When blended recycled flame retardant, antibacterial and low-melting-point PET is used as the cortex in Comparative Examples 2 and 4, the roughness of the fabric is higher than that in Examples 1 to 4, and even higher than that of the ordinary PET cortex. The above results indicate that the chemically regenerated flame retardant, antibacterial and low-melting-point cotton fiber provided in the present application has higher softness and a better fabric feel.
[0053] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A chemically regenerated flame-retardant and antibacterial low-melting cotton fiber, characterized in that: The cotton fiber is a skin-core structure, the raw material of the core layer of the skin-core structure is copolymerized flame-retardant PET, the raw material of the skin layer of the skin-core structure is recycled flame-retardant antibacterial low-melting-point PET, and the recycled flame-retardant antibacterial low-melting-point PET is copolymerized with quaternary ammonium salt and PET waste alcoholysis product as raw materials.
2. The chemically regenerated flame-retardant and antibacterial low-melting cotton fiber according to claim 1 is characterized in that: The quaternary ammonium salt is a quaternary ammonium salt of a long-chain alkyl naphthol derivative.
3. The chemically regenerated flame-retardant, antibacterial, low-melting cotton fiber according to claim 1 or 2, characterized in that: The quaternary ammonium salt is prepared by reacting chloroacetyl organic amine and long-chain alkyl naphthol derivative.
4. The chemically regenerated flame-retardant and antibacterial low-melting cotton fiber according to claim 3 is characterized in that: The long-chain alkyl naphthol derivative is prepared by alkylation reaction of organic amine and long-chain olefin.
5. The chemically regenerated flame-retardant and antibacterial low-melting cotton fiber according to claim 1 is characterized in that: The alcoholysis product of the PET waste includes one or more of regenerated terephthalic acid, regenerated dimethyl terephthalate, regenerated ethylene terephthalate and ethylene glycol.
6. A method for preparing chemically regenerated flame-retardant, antibacterial, low-melting cotton fibers according to any one of claims 1 to 5, characterized in that: The following steps are involved: Step 1: performing an alkylation reaction on an organic amine and a long-chain olefin under the action of a catalyst to prepare a long-chain alkyl naphthol derivative, and adding the long-chain alkyl naphthol derivative and a chloroacetyl organic amine into a solvent for reaction to prepare a quaternary ammonium salt of the long-chain alkyl naphthol derivative; Step 2: Screening and crushing the PET polyester waste to obtain PET waste fragments, heating the PET waste fragments until they are melted, adding diol and a catalyst to perform primary alcoholysis and secondary alcoholysis respectively to obtain PET waste alcoholysis products, and uniformly mixing the PET alcoholysis products and a quaternary ammonium salt of a long-chain alkyl naphthol derivative to perform esterification reaction and polycondensation reaction to prepare a regenerated flame-retardant, antibacterial, low-melting-point PET; Step 3: adding 1,2-dicarboxyethyldiphenylphosphine oxide, terephthalic acid, ethylene glycol, a catalyst and a stabilizer into a container to respectively carry out esterification reaction and polycondensation reaction to prepare a copolymer flame-retardant PET; Step 4: After drying, the copolymerized flame-retardant PET and the regenerated flame-retardant antibacterial low-melting-point PET are injected into a melt spinning device for skin-core composite spinning to produce chemically regenerated flame-retardant antibacterial low-melting cotton fibers.
7. The preparation method according to claim 6, characterized in that: In the step 1, the molar ratio of the organic amine to the long-chain olefin is 3-6:
1.
8. The preparation method according to claim 6 or 7, characterized in that: The diol in step 2 is one or more of ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butylene glycol, 1,4-butylene glycol, 1,5-pentanediol, 2,2-dimethyl-1,3-propylene glycol, 2-ethyl-2-tert-butyl-1,3-propylene glycol or 2,2,4-trimethyl-1,6-hexanediol.
9. The preparation method according to claim 6, characterized in that: The catalyst in step 2 is zinc acetate.
10. The preparation method according to claim 9, characterized in that: The amount of zinc acetate used is 0.5-1.5 wt%.