PVDF / CNT-coated PVDF / PTFE composite nanofiber membrane as well as preparation method and application thereof

Through the preparation of PVDF/CNT@PVDF/PTFE composite nanofiber membrane, the shortcomings of existing wearable strain sensors in terms of mechanical performance, thermal stability and sensitivity are solved, and the efficient working ability in harsh environments is achieved. It is suitable for multiple applications. A kind of application scenario.

CN119083032AActive Publication Date: 2024-12-06NANJING TECH UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411214097.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-31
Publication Date
2024-12-06
Estimated Expiration
2044-08-31

AI Technical Summary

Technical Problem

Existing wearable strain sensors have shortcomings in mechanical properties, thermal stability and sensitivity, and are not adaptable to harsh environments, making it difficult to maintain efficient work for a long time.

Method used

Using the preparation method of PVDF/CNT@PVDF/PTFE composite nanofiber membrane, PVDF, CNT and PTFE are dissolved in a specific solvent to form a nanofiber membrane with a core-shell structure, and CNT is coated on the surface of the fiber membrane to enhance its conductivity. and thermal stability, forming a modified PVDF/CNT@PVDF/PTFE composite nanofiber membrane for the preparation of wearable strain sensors.

Benefits of technology

Improves the mechanical properties, thermal stability and sensitivity of wearable strain sensors, enhances the adaptability to harsh environments, and maintains good resistance response and stability under high temperatures and different strain conditions. It is suitable for use in a variety of application scenarios .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119083032A_ABST
    Figure CN119083032A_ABST
Patent Text Reader

Abstract

The invention provides a PVDF / CNT-coated PVDF / PTFE composite nanofiber membrane as well as a preparation method and application thereof, and belongs to the technical field of electrostatic spinning. The performance of the fiber membrane is greatly improved by adding the CNT particles and the PTFE; and the two components are made into a core-shell structure, so that the advantageous properties of the two materials can be utilized to the greatest extent, and meanwhile, the core-shell structure can also improve the properties of the fiber membrane. The dispersed CNT solution is coated on the surface of the nanofiber membrane for modification, so that the thermal stability and the sensitivity of the PVDF / CNT-coated PVDF / PTFE composite nanofiber membrane can be further enhanced. The wearable strain sensor prepared by using the PVDF / CNT-coated PVDF / PTFE composite nanofiber membrane disclosed by the invention has the advantages of high mechanical property, high thermal stability and high sensitivity, is environment-friendly, and has the capability of working in a severe environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrostatic spinning, and in particular to a PVDF / CNT@PVDF / PTFE composite nanofiber membrane and a preparation method and application thereof. Background Art

[0002] Artificial smart fabrics can harvest a variety of biomechanical energies from human motion and effectively convert them into stable electrical energy. Using artificial smart fabrics to prepare wearable strain sensors is an effective way to sustainably drive wearable electronic devices in a clean, safe and efficient manner. In addition to the energy harvesting function, these smart fabrics can also be integrated with everyday clothes to sense the amplitude of human motion and serve as highly sensitive sensors for human motion and posture. These characteristics also provide a basis for the widespread application of artificial smart fabrics in smart textiles and the next generation of wearable electronics.

[0003] In recent years, many experts and scholars have published articles on wearable strain sensors, but they all have certain limitations and cannot maintain good mechanical and thermal stability. Some are also greatly affected by harsh environments. Therefore, building smart textiles that can generate electricity through human mechanical movement is a good solution and an important step forward in achieving fully wearable power in a clean, safe and sustainable way. Summary of the invention

[0004] The purpose of the present invention is to provide a PVDF / CNT@PVDF / PTFE composite nanofiber membrane and a preparation method and application thereof. The wearable strain sensor prepared using the PVDF / CNT@PVDF / PTFE composite nanofiber membrane of the present invention has high mechanical properties, thermal stability and sensitivity, is environmentally friendly, and has the ability to work in harsh environments.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a method for preparing a PVDF / CNT@PVDF / PTFE composite nanofiber membrane, comprising the following steps:

[0007] (1) dissolving PVDF and CNT in DMF and acetone to obtain a first solution;

[0008] (2) dissolving the PVDF and PTFE concentrated solutions in a mixed solution of DMF and acetone to obtain a second solution;

[0009] (3) preparing a nanofiber membrane: the first solution and the second solution are coaxially connected, placed in a spinning device, woven to form a core-shell structure, wherein the core layer is PVDF / PTFE and the shell layer is PVDF / CNT, the woven structure is placed in a receiving device, taken out from the receiving device, and dried to obtain a nanofiber membrane;

[0010] (4) Nanofiber membrane modification: CNTs are dispersed in a solvent, coated on the surface of the nanofiber membrane, and dried to obtain a modified PVDF / CNT@PVDF / PTFE composite nanofiber membrane.

[0011] Furthermore, in step (1), the mass ratio of PVDF, CNT, DMF and acetone is PVDF: CNT: DMF: acetone = 1-2 g: 0.001-0.1 g: 3-6 mL: 1-3 mL.

[0012] Furthermore, in step (2), the mass volume ratio of PVDF, PTFE, DMF and acetone is: PVDF:PTFE:DMF:acetone=1-2g:50-150μL:3-6mL:1-3mL; the concentration of PTFE is 60%.

[0013] Furthermore, in step (3), the volume ratio of the first solution to the second solution is 1-2:1-2; and a layer of attachment is attached to the receiving device.

[0014] Furthermore, in step (4), the mass volume ratio of CNT to solvent is 0.025-0.1 g:6-24 mL; the solvent is one of ethanol, DMF, and PVP; the coating amount is 0.5-1.5 g / m 2 , coating includes drop coating or spin coating.

[0015] The present invention also provides a PVDF / CNT@PVDF / PTFE composite nanofiber membrane prepared by a method for preparing the PVDF / CNT@PVDF / PTFE composite nanofiber membrane.

[0016] The present invention also provides an application of a PVDF / CNT@PVDF / PTFE composite nanofiber membrane in the preparation of a wearable strain sensor.

[0017] Furthermore, the method for preparing the wearable strain sensor is:

[0018] The two ends of the PVDF / CNT@PVDF / PTFE composite nanofiber membrane were connected to the electrodes and fixed with conductive silver paste to obtain a wearable strain sensor.

[0019] Furthermore, the electrode includes a conductive tape, a thin copper wire or a fiber film.

[0020] The beneficial effects of the present invention compared with the prior art are:

[0021] (1) CNT has excellent electrical conductivity, mechanical properties, flexibility and heat transfer properties. PTFE is known as the king of plastics and has good chemical stability, corrosion resistance, sealing and high lubricity and non-stickiness. The present invention greatly improves the performance of the fiber membrane by adding CNT particles and PTFE; and the two components are made into a core-shell structure, which can maximize the advantages of the two materials. At the same time, the core-shell structure can also improve the performance of the fiber membrane. The dispersed CNT solution is coated on the surface of the nanofiber membrane for modification, which can further enhance the thermal stability and sensitivity of the PVDF / CNT@PVDF / PTFE composite nanofiber membrane.

[0022] (2) When preparing the PVDF / CNT@PVDF / PTFE composite nanofiber membrane, the present invention can attach attachments of different properties to the receiving device, which greatly increases the application range of the nanofiber membrane.

[0023] (3) When preparing a wearable strain sensor, the present invention can change the electrodes of the sensor according to different needs, which greatly increases the application field of the wearable strain sensor. The prepared wearable strain sensor has high mechanical properties, thermal stability and sensitivity, is environmentally friendly, and has the ability to work in harsh environments. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0025] Figure 1 This is a SEM image of the PVDF / CNT@PVDF / PTFE composite nanofiber membrane prepared in Example 1;

[0026] Figure 2 This is a thermal stability test of the PVDF / CNT@PVDF / PTFE composite nanofiber membrane prepared in Example 1, wherein A is the sample of the present invention, B is the PVDF / MWCNTs@PVDF / PTFE nanofiber membrane; and C is the PVDF / MWCNTs nanofiber membrane;

[0027] Figure 3 The resistance response of the PVDF / CNT@PVDF / PTFE composite nanofiber membrane prepared in Example 1 under different stretching voltages;

[0028] Figure 4The resistance response of the PVDF / CNT@PVDF / PTFE composite nanofiber membrane prepared in Example 1 under different strains;

[0029] Figure 5 The resistance response of the wearable strain sensor prepared in Example 1 before and after being immersed in water for 24 hours;

[0030] Figure 6 The resistance response of the wearable strain sensor prepared in Example 1 after cutting;

[0031] Figure 7 The wearable strain sensor prepared in Example 1 is used to test the resistance response of pulse beating;

[0032] Figure 8 The cyclic stability of the wearable strain sensor prepared in Example 1;

[0033] Fig. 9 This is a schematic diagram of the structure of the wearable strain sensor prepared in Example 1. DETAILED DESCRIPTION

[0034] The embodiments of the present invention are described in detail below, and the embodiments are intended to explain the present invention and should not be construed as limiting the present invention. If specific techniques or conditions are not specified in the embodiments, they are carried out according to the techniques or conditions described in the literature in this area or according to the product specifications. If the manufacturers of reagents or instruments are not specified, they are all conventional products that can be obtained commercially.

[0035] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0036] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0037] The present invention provides a PVDF / CNT@PVDF / PTFE composite nanofiber membrane, which specifically comprises the following steps:

[0038] (1) Dissolving PVDF and CNT in a mixed solution of DMF and acetone to obtain a first solution; wherein PVDF: CNT: DMF: acetone = 1-2 g: 0.001-0.1 g: 3-6 mL: 1-3 mL, and most preferably 1 g: 0.005 g: 3.315 g: 1.42 g.

[0039] (2) Dissolving the concentrated PVDF and PTFE solution in a mixed solution of DMF and acetone to obtain a second solution; wherein PVDF:PTFE:DMF:acetone=1-2 g:50-150 μL:3-6 mL:1-3 mL, and most preferably 1 g:50 μL:3.315 g:1.42 g; and the concentration of the PTFE is 60%.

[0040] The first solution and the second solution are both heated and stirred until they are uniform, wherein the heating includes magnetic vibration heating or ultrasonic vibration heating.

[0041] (3) preparing a nanofiber membrane: the first solution and the second solution are coaxially connected, placed in a spinning device, woven to form a core-shell structure, wherein the core layer is PVDF / PTFE and the shell layer is PVDF / CNT, and the woven structure is placed in a receiving device, taken out from the receiving device, and then vacuum dried to remove residual solvent to obtain a nanofiber membrane;

[0042] The spinning device comprises a receiving device, a coaxial mechanism, a high-voltage power supply, and an injection pump, wherein the receiving device comprises a roller; and a layer of attachment is attached to the receiving device.

[0043] (4) Nanofiber membrane modification: The prepared fiber membrane is taken out and cut, CNT is dispersed in a solvent, coated on the surface of the nanofiber membrane, and vacuum dried to obtain a modified PVDF / CNT@PVDF / PTFE composite nanofiber membrane;

[0044] The solvent is one of ethanol, DMF and PVP; the dispersion method is: first magnetic stirring for 5 hours, and then ultrasonic oscillation for 1 to 2 hours; the modification is to coat the dispersed CNT solution on the fiber surface, the coating includes drop coating or spin coating, or placing the cut fiber membrane into the solution for ultrasonic oscillation; the coating amount is 0.5 to 1.5 g / m 2 .

[0045] The present invention provides a method for preparing a wearable strain sensor using a PVDF / CNT@PVDF / PTFE composite nanofiber membrane, which specifically comprises the following steps:

[0046] (5) Connecting both ends of the PVDF / CNT@PVDF / PTFE composite nanofiber membrane to electrodes and fixing them with conductive silver paste; wherein the electrodes can be thin copper wires or other types of fiber membranes.

[0047] Example 1

[0048] Embodiment 1 of the present invention provides a method for preparing a wearable strain sensor, which specifically comprises the following steps:

[0049] (1) 0.005 g of CNT particles and 1 g of PVDF powder were dissolved in a mixed solution obtained by mixing 3.315 mL of DMF and 1.42 mL of acetone, and then magnetically stirred at room temperature for 6 h and ultrasonically vibrated for 2 h until the mixture was uniformly dispersed to obtain a first solution;

[0050] (2) 50 μL of PTFE concentrate and 1 g of PVDF were dissolved in a mixed solution obtained by mixing 3.315 mL of DMF and 1.42 mL of acetone, and then magnetically stirred at 60° C. for 6 h until the solution was uniformly dispersed, thereby obtaining a second solution.

[0051] (3) Take two clean syringes with a volume of 5 mL, draw the first solution and the second solution into the syringes respectively, and then connect the two syringes with a special coaxial needle. The second solution is ejected from the inner needle as the core layer material, and the first solution is ejected from the outer needle as the shell layer material.

[0052] Then set the parameters: the distance between the receiving device and the nozzle is 12.5 cm, the voltage is 20 kV, the feed speed of the main pump and the auxiliary pump is 0.0007 mm / s, the relative humidity is about 60%, the temperature is about 25 ° C, cover the drum with a layer of tin foil to receive the fiber, and finally start spinning to obtain a fiber membrane. The obtained fiber membrane is placed in a vacuum drying oven and dried for 2 hours. The temperature is set to 70 ° C to remove residual solvent. The dried fiber membrane is taken out and cut into 7 cm*4 cm rectangular samples to obtain a nanofiber membrane.

[0053] (4) 0.025 g of CNT particles were dispersed in 6 ml of ethanol solution, first magnetically stirred at room temperature for 10 min, then ultrasonically shaken for 2 h, during which the water was changed every half an hour to ensure the water temperature was balanced, and finally the dispersed CNT was coated on the prepared sample. The coating amount was 1.5 g / m 2 The modified PVDF / CNT@PVDF / PTFE composite nanofiber membrane was then dried at 60°C for 1 h.

[0054] (5) Conductive tape was pasted on both sides of the PVDF / CNT@PVDF / PTFE composite nanofiber membrane to act as an electrode, and conductive silver paste was coated between the conductive tape and the fiber membrane, and then dried at 60 °C for 1 h to obtain a wearable strain sensor.

[0055] The prepared wearable strain sensor was tested for performance, such as sensitivity, mechanical properties, thermal stability, etc. Figures 1 to 8 As shown, its structure diagram is as follows Fig. 9 shown.

[0056] from Figure 1It can be seen that all the fibers in the fiber membrane show random orientation, the fiber surfaces are smooth and flat, and they are naturally stacked with each other to form a 3D porous network structure. In addition, since a layer of MWCNTs is coated on the fiber surface, there are a large number of particles bonded to the fiber surface, which directly indicates that the coating of MWCNTs is successful.

[0057] Figure 2 The shrinkage of three different fiber membranes (sample size: a circle with a diameter of 3.5 cm) after standing for 30 minutes at 140°C, 160°C, and 180°C was compared. At 140°C, it can be seen that the three fiber membranes remain in their original state and the morphology has basically not changed. At 160°C, the sample fiber membrane of the present invention still does not change much, while the uncoated PVDF / MWCNTs@PVDF / PTFE fiber membrane has some smaller curling and some warping on the edges, but the overall morphology has not changed much, while the PVDF / MWCNTs fiber membrane has obvious wrinkles and shrinkage. At 180°C, the sample fiber membrane of the present invention can still maintain a good morphology, the uncoated PVDF / MWCNTs@PVDF / PTFE fiber membrane has obvious curling, and the curling of the PVDF / MWCNTs fiber membrane is more obvious, and even the edge of the fiber membrane has serious shrinkage, resulting in a huge change in the overall morphology of the fiber membrane. Therefore, it can be seen that the sample fiber membrane of the present invention has good heat resistance, can maintain good fiber morphology at 180°C, and basically does not curl or shrink.

[0058] Figure 3 It can be seen that the flexible strain sensor assembled from the sample fiber membrane of the present invention has good stability and repeatability in the resistance response of the sensor at different stretching rates, and the waveform is also stable and normal. The resistance response at different stretching rates is stable at about 2.5, 2.7 and 4.2, respectively, and the curve fluctuation frequency is also increasing with the increase of the stretching rate in the same time. It can be seen from the figure that the resistance response value is also increasing with the increase of the stretching rate. This is because the greater the stretching rate, the greater the deformation of the sensor, that is, the fiber is stretched, thereby increasing the real-time resistance of the fiber, and the change of the fiber resistance will directly affect the real-time resistance of the sensor. At the same time, the response time is relatively stable, and the stability of the response time can be increased without affecting the increase of the stretching frequency.

[0059] from Figure 4It can be seen that the sensor assembled from the sample fiber membrane of the present invention has good stability and repeatability, and the resistance response value also increases with the increase of strain in the same time. And it can be seen from the figure that as the tensile strain increases, the resistance response value also increases continuously, because the greater the tensile strain, the greater the deformation of the sensor, and thus the greater the change in the resistance response value. The resistance response value increases from 2.2 to about 8.3, and the resistance response value maintains good stability under each strain.

[0060] from Figure 5 It can be seen that the sensor assembled from the sample fiber membrane of the present invention shows better stability and repeatability, the resistance response value is stable at about 1.5, the waveform has an obvious fluctuation pattern, and there is no slow change of the waveform. However, after 24 hours of immersion, the resistance response value has a slight decrease and stabilizes at about 1.3. This is because the hydrophobicity of the composite fiber membrane coated with MWCNTs is slightly poor, which has a slight impact on the sensor after immersion. However, it can also be seen from the figure that this impact is negligible and basically does not affect the normal use of the sensor.

[0061] from Figure 6 It can be seen that the sensor assembled from the sample fiber membrane of the present invention has a stable waveform and good repeatability. The resistance response values ​​before and after cutting are stable between 1.8-1.9, and the waveform changes before and after cutting have very obvious regularity. At the same time, the transition at the node of stretching and releasing is very smooth, without any delay, which means that the sensor assembled from the composite fiber membrane has good cutability and high sensitivity, and can be cut into different shapes according to actual needs. At the same time, the time response is very stable and can be kept within a certain range.

[0062] Figure 7 The waveform diagram for testing pulse beats shows that the test results are completely consistent with the normal pulse beats per minute (60-100 times / min), and have good stability and repeatability. The resistance response value is stable at around 1.002. The resistance response value is very low because the pulse beats cannot cause a large deformation of the sensor. However, from the waveform diagram, it can be seen that there is still a slight gap in the waveform. This is because the skin at the wrist may vibrate slightly during the test, and the test environment may cause errors.

[0063] Figure 8This is a cyclic stability test diagram of the sensor, and the test speed is 1 cycle / s. It can be seen from the figure that after 40,000 stretch releases, it still has good stability and repeatability. It can also be seen that the change in the waveform has good stability and repeatability, and the resistance response has always remained at around 20, indicating that the sensor prepared by the present invention has a long service life and can maintain good stability in long-term work. However, it can also be seen from the figure that some waveforms have certain defects. This is because the test equipment is placed in the air and the test time is long, resulting in certain errors, which is a normal phenomenon.

[0064] Fig. 9 This is a schematic diagram of the structure of the sensor. The prepared solution was sucked out with a syringe, and then a PVDF / MWCNTs@PVDF / PTFE nanofiber membrane with a core-shell structure was prepared by coaxial electrospinning. A layer of MWCNTs was coated on the surface of the fiber membrane, and then a conductive tape was connected as an electrode, and finally encapsulated by PDMS.

[0065] Example 2

[0066] Example 2 of the present invention adopts the preparation method of the wearable strain sensor of Example 1 to prepare a wearable strain sensor. The difference from Example 1 is that in Example 2, a layer of conductive fabric is covered on the roller of the receiving device for directly receiving fibers, which can further improve the conductivity.

[0067] Example 3

[0068] Example 3 of the present invention adopts the preparation method of the wearable strain sensor of Example 1 to prepare a wearable strain sensor. The difference from Example 1 is that in Example 3, the prepared fiber membrane is immersed in dispersed CNTs, and then ultrasonically vibrated for 1 hour, so that the CNTs can be well adsorbed on the fiber surface.

[0069] Example 4

[0070] A wearable strain sensor was prepared by adopting the preparation method of the wearable strain sensor of Example 4. The difference from Example 1 is that Example 4 uses other types of fiber membranes as electrodes, which are then led out with copper wires. It can be used as a nano friction generator, which greatly increases the application field.

[0071] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a PVDF / CNT@PVDF / PTFE composite nanofiber membrane, characterized in that: The steps include: (1) dissolving PVDF and CNT in a mixed solution of DMF and acetone to obtain a first solution; (2) dissolving the PVDF and PTFE concentrated solutions in a mixed solution of DMF and acetone to obtain a second solution; (3) preparing a nanofiber membrane: the first solution and the second solution are coaxially connected, placed in a spinning device, woven to form a core-shell structure, wherein the core layer is PVDF / PTFE and the shell layer is PVDF / CNT, the woven structure is placed in a receiving device, taken out from the receiving device, and dried to obtain a nanofiber membrane; (4) Nanofiber membrane modification: CNTs are dispersed in a solvent, coated on the surface of the nanofiber membrane, and dried to obtain a modified PVDF / CNT@PVDF / PTFE composite nanofiber membrane.

2. The method for preparing the PVDF / CNT@PVDF / PTFE composite nanofiber membrane according to claim 1, characterized in that: In step (1), the mass volume ratio of PVDF, CNT, DMF and acetone is PVDF: CNT: DMF: acetone = 1-2 g: 0.001-0.1 g: 3-6 mL: 1-3 mL.

3. The method for preparing the PVDF / CNT@PVDF / PTFE composite nanofiber membrane according to claim 1, characterized in that: In step (2), the mass volume ratio of PVDF, PTFE, DMF and acetone is: PVDF:PTFE:DMF:acetone=1-2g:50-150μL:3-6mL:1-3mL; the concentration of PTFE is 60%.

4. The method for preparing the PVDF / CNT@PVDF / PTFE composite nanofiber membrane according to claim 1, characterized in that: In step (3), the volume ratio of the first solution to the second solution is 1-2:1-2; and a layer of attachment is attached to the receiving device.

5. The method for preparing the PVDF / CNT@PVDF / PTFE composite nanofiber membrane according to claim 1, characterized in that: In step (4), the mass volume ratio of CNT to solvent is 0.025-0.1 g:6-24 mL; the solvent is one of ethanol, DMF, and PVP; the coating amount is 0.5-1.5 g / m 2 , coating includes drop coating or spin coating.

6. A PVDF / CNT@PVDF / PTFE composite nanofiber membrane prepared by the method for preparing a PVDF / CNT@PVDF / PTFE composite nanofiber membrane according to any one of claims 1 to 5.

7. Use of the PVDF / CNT@PVDF / PTFE composite nanofiber membrane according to claim 6 in the preparation of a wearable strain sensor.

8. The use of the PVDF / CNT@PVDF / PTFE composite nanofiber membrane in the preparation of a wearable strain sensor according to claim 7, characterized in that: The method for preparing the wearable strain sensor is: The two ends of the PVDF / CNT@PVDF / PTFE composite nanofiber membrane were connected to the electrodes and fixed with conductive silver paste to obtain a wearable strain sensor.

9. The use of the PVDF / CNT@PVDF / PTFE composite nanofiber membrane in the preparation of a wearable strain sensor according to claim 8, characterized in that: The electrodes include conductive tapes, thin copper wires or fiber films.

Citation Information

Patent Citations

  • Preparation method of polyvinylidene fluoride (PVDF) / carbon nanotube composite nanofibers

    CN102719927A

  • Fiber-based shape adaptive passive electronic skin and preparation method thereof

    CN110274713A

  • Composite nanofiber membrane as well as preparation method and application thereof

    CN115976740A

  • Method for preparing flexible inorganic / organic nanofiber integrated composite membrane

    CN117569002A

  • Cleanable flexible multifunctional coaxial electrospun fibrous membrane as well as preparation and application thereof