Sensing layer and preparation method thereof, sensor made of sensing layer and preparation method of sensor

Through high-energy plasma treatment and chemical graft modification, the hydrophilic surface is formed, combined with electrostatic self-assembly and thermoforming processes, the problem of MXene flexible pressure sensor being susceptible to damage and poor stability under mechanical stress is solved, and the detection accuracy and sensitivity are improved. The detection range has been expanded and mechanical properties have been enhanced.

CN119085897AActive Publication Date: 2024-12-06GUILIN UNIV OF ELECTRONIC TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411201281.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

MXene flexible pressure sensor is susceptible to damage and peeling under mechanical stress. The interlayer contact resistance of the device affects detection accuracy, poor stability and durability, insufficient flexibility and mechanical properties, and limited sensitivity and detection range.

Method used

The hydrophilic surface is formed through high-energy plasma treatment and chemical grafting modification, and the metal nanowire network is prepared by electrostatic self-assembly and thermoforming processes to improve the binding force between MXene and flexible substrate, reduce interface impedance, and enhance mechanical structure strength and sensitivity.

Benefits of technology

It improves the stability and detection accuracy of the sensor, enhances flexibility and mechanical properties, expands the detection range and sensitivity, and reduces the electrical impedance and oxidation risks of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119085897A_ABST
    Figure CN119085897A_ABST
Patent Text Reader

Abstract

The invention provides a sensing layer and a preparation method thereof, and a sensor prepared from the sensing layer and a preparation method thereof, and belongs to the technical field of sensors, and the preparation method of the sensor comprises the following steps: S1, processing a flexible substrate: carrying out degreasing, blow-drying and dehydration on a bearing plate spin-coated with a PDMS mixed solution, then bombarding the PDMS surface with inert gas high-energy plasma, and drying the bearing plate; carrying out oxygen plasma cleaning on the obtained PDMS flexible substrate to obtain a hydroxylated PDMS flexible substrate, dipping the hydroxylated PDMS flexible substrate in a PVA solution, carrying out blow-drying, then carrying out heating, and repeating the dipping-drying steps for many times to obtain a treated PDMS flexible substrate; and S2, modifying the treated PDMS flexible substrate to prepare a surface metal layer. Therefore, by adopting the sensing layer and the preparation method thereof, the sensor prepared from the sensing layer and the preparation method thereof, the problems of poor stability, poor sensitivity, low recognition precision, small detection range and low mechanical property in the prior art are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of sensor technology, and in particular to a sensing layer and a preparation method thereof, a sensor made of the sensing layer and a preparation method thereof. Background Art

[0002] With the rapid rise of artificial intelligence and Internet of Things technologies, flexible wearable sensors have aroused widespread research enthusiasm in recent years and can be widely used in health management, medical diagnosis and other fields. Flexible pressure sensors can effectively convert mechanical signals into electrical signals, intuitively detect and reflect complex human physiological and posture signals, and change with the deformation of materials and external pressure, showing great commercial value in disease diagnosis and health care in medical institutions. MXene is considered to be one of the most promising sensing materials because of its metal-like conductivity, excellent dispersibility, and especially its large resistance change under external force. However, there are still some shortcomings in the research of MXene flexible pressure sensors:

[0003] ① Combination with substrate: MXene usually needs to be combined with a flexible substrate to prepare a flexible pressure sensor. However, the interfacial adhesion between MXene nanosheets and the flexible substrate is poor, so during the continuous movement of the limbs, the sensing layer is easily damaged or even peeled off when it is constantly subjected to mechanical stress.

[0004] ② Contact resistance between device layers: Current research only focuses on the electrical properties of the force-sensitive sensing layer of flexible sensors, but ignores the impact of contact resistance between device layers on detection accuracy.

[0005] ③ Stability and durability: MXene may encounter stability and durability issues in flexible pressure sensors. Since MXene itself is sensitive to water and oxygen, it may degrade after long-term use or in complex environments, resulting in decreased sensor performance.

[0006] ④Flexibility and mechanical properties: Although MXene itself has good mechanical strength, the flexibility of flexible pressure sensors still needs to be improved. Especially under a wide range of bending or tensile strain, the performance of the sensor may be affected, resulting in reduced reliability and stability.

[0007] ⑤ Sensitivity and detection range: Although MXene has good electrical conductivity and mechanical strength, it is prone to self-stacking due to the existence of van der Waals forces, and the sensitivity and detection range of flexible pressure sensors can still be further improved. Current MXene pressure sensors may have limitations in detecting smaller pressure changes or pressure changes over a wider range. Summary of the invention

[0008] In order to solve the above problems, the present invention provides a sensing layer for a sensor, the sensor and a preparation method thereof, so as to avoid the problem that each specification of staircase molds in the prior art cannot be used for the production of stairs of other specifications, causing great waste.

[0009] The present invention provides a method for preparing a sensing layer, comprising the following preparation steps:

[0010] S1. Spin-coat the PDMS mixture on the carrier plate, then degrease, blow dry, dehydrate, bombard the PDMS surface with inert gas high-energy plasma, and clean the obtained PDMS flexible substrate with oxygen plasma to obtain a hydroxylated PDMS flexible substrate, immerse the hydroxylated PDMS flexible substrate in a PVA solution, blow dry and heat, and repeat the immersion-drying steps several times to obtain a treated PDMS flexible substrate;

[0011] S2. Modify the treated PDMS flexible substrate to prepare a surface metal layer.

[0012] Preferably, the MXene / microsphere ink is sprayed onto the treated surface of the PDMS flexible substrate. After the spraying is completed, the PDMS flexible substrate with the MXene / microsphere coating is pyrolyzed to remove the microspheres to obtain a flexible substrate with a MXene film deposited. The flexible substrate with the MXene film deposited is then placed in a solution of metal ions, and metal nanowires are grown on the MXene coating to obtain a surface metal layer.

[0013] Preferably, during the spraying process, the water in the MXene / microsphere ink is ensured to evaporate before each spraying, and the spraying is repeated multiple times until the MXene / microsphere deposition amount is about 0.1-0.3 mg / cm 2 The steps of pyrolysis to remove microspheres are as follows: after spraying, the PDMS flexible substrate with MXene / microsphere coating is placed in a drying oven to dry, and then pyrolysis is performed in a vacuum sintering furnace to remove the microspheres. Under the protection of inert gas, the pyrolysis treatment is performed at a high temperature of 350-500°C for 13-20 minutes to burst the microspheres inside the coating, leaving hollow holes inside. Before high-temperature pyrolysis, the vacuum sintering furnace is repeatedly filled with inert gas to exclude oxygen. The heating temperature of the vacuum sintering furnace is controlled at above 100°C / minute to prevent the microspheres from melting due to heat.

[0014] The present invention provides a sensing layer manufactured according to the above-mentioned method for manufacturing the sensing layer.

[0015] The present invention provides a sensor, comprising a sensing layer made by the sensing layer preparation method.

[0016] The present invention provides a method for preparing a sensor, comprising the following preparation steps:

[0017] S1. prepare a microsphere dispersion and a MXene solution respectively, add the microsphere dispersion dropwise into the MXene solution for electrostatic self-assembly, slowly stir the mixed MXene / microsphere dispersion, during which the negatively charged MXene nanosheets are wrapped on the surface of the microspheres by electrostatic self-assembly, and concentrate after stirring to obtain the MXene / microsphere ink to be prepared;

[0018] S2. Prepare the sensing layer;

[0019] S3. Preparation of flexible electrode film: using a flexible film as a substrate, spraying photoresist uniformly on the obtained flexible substrate, drying and curing the photoresist on the flexible film with photoresist, and printing the required interdigitated electrode pattern on a film as a mask using an inkjet printer; placing the pattern surface of the mask close to the cured photoresist coating, and removing the photoresist on the patterned part after ultraviolet exposure; cleaning the obtained sample with argon and oxygen plasma, and magnetron sputtering a titanium layer, a copper layer, and a gold layer on the surface in sequence; removing the remaining photoresist and the metal layer thereon with a release agent to obtain a patterned interdigitated electrode layer;

[0020] S4. Assembly: Use copper wire to connect the two electrodes of the interdigital electrode through conductive silver paste to establish an external circuit, apply PDMS on the top layer as a fixing agent, treat the flexible substrate and the sensing layer and flexible electrode film obtained in the above steps with oxygen plasma, and vertically plane-laminate in the order of encapsulation layer - electrode layer - sensing layer - flexible substrate - encapsulation layer; the encapsulation layer is a flexible film.

[0021] Preferably, the specific steps for preparing the microsphere dispersion are: dispersing the prepared microsphere solution in a cationic polymer polydiallyl dimethyl ammonium chloride solution PDDA by ultrasonic treatment to obtain a mixture, stirring the mixture, filtering it with an aqueous filter membrane, and washing it with deionized water to remove the cationic polymer polydiallyl dimethyl ammonium chloride solution PDDA, and re-dispersing the microspheres on the aqueous filter membrane in deionized water to obtain a positively charged microsphere dispersion; the specific steps for preparing the MXene solution are: dissolving the MXene powder in water, ultrasonicating for 20-40 minutes under the protection of an inert gas to obtain a MXene dispersion, and then centrifuging the MXene dispersion to obtain the supernatant, which is the MXene solution.

[0022] Preferably, the microspheres are one or more of polystyrene microspheres, polymethyl methacrylate microspheres, polystyrene-co-acrylate copolymer microspheres, and polylactic acid microspheres, and the average diameter of the microspheres is 0.5-2 μm.

[0023] Preferably, in step S1, during electrostatic self-assembly, the mass ratio of microspheres to MXene is 1:2;

[0024] The material of the flexible film in step S3 and step S4 is a flexible insulating material, which is one or more of polyimide, polyethylene terephthalate, polyethylene naphthalate, polymethyl methacrylate and polyurethane; preferably, the flexible film is polyimide.

[0025] When the PDMS surface is treated with high-energy inert gas plasma, the PDMS surface is bombarded by ions with high energy. These ions can cause a certain degree of surface deformation and cutting when they hit the PDMS surface, forming a micro-gap structure. Due to ion bombardment, the molecular structure of the PDMS surface may be rearranged. Microstructures or nanostructures are formed, thereby increasing the roughness of the surface. The rough surface has a larger surface area, so it can enhance the interaction between PDMS and MXene.

[0026] Oxygen plasma bombardment destroys the non-polar methyl groups (-CH3) on the PDMS surface and produces polar groups such as hydroxyl (-OH), carboxyl (-COOH) and silanol (-SiOH). These functional groups can form hydrogen bonds with highly polar PVA molecules to form a hydrophilic surface. In addition, the layered structure of MXene facilitates its better adhesion to the PVA surface, and the functional groups on the MXene surface can form strong hydrogen bonds with the hydroxyl (-OH) in the PVA chain. In addition, the van der Waals force of MXene also further promotes its adhesion to a certain extent.

[0027] Metal nanowires are grown in situ on the MXene coating; the metal layer composed of crossed metal nanowires increases the conductive layer area of ​​the MXene force-sensitive sensing layer. Due to the gaps in the MXene coating, the metal nanowires can grow and penetrate into the sub-surface layer of the MXene coating to form a conductive network, reducing the interface impedance value of the MXene coating, and the porous grid structure of the MXene coating is also conducive to forming an electronic barrier, reducing the loss of electrons inside the electrode, thereby further reducing the interface impedance value of the force-sensitive sensing layer. The presence of the metal electrode layer composed of crossed metal nanowires and the MXene coating greatly reduces the electrical impedance of the flexible electrode and improves its stretching function.

[0028] Therefore, the present invention provides the above-mentioned sensing layer and preparation method, sensor made of the sensing layer and preparation method thereof, which have the following beneficial effects:

[0029] 1) In response to the problem mentioned in the background technology that the sensing layer is easily damaged and peeled off when subjected to mechanical stress, the present invention reduces the surface energy of the PDMS flexible substrate through the synergistic effect of physical micro-gap structure micro-nano processing (high-energy plasma treatment) and chemical grafting modification (PVA), so that the PVA molecules and the activated PDMS surface undergo hydrogen bonding to form a hydrophilic surface, so that MXene and PDMS are combined through a chemical grafting method. Compared with traditional solutions such as oxygen plasma cleaning, silane coupling agent surface modification, and UV irradiation, the present invention has strong bonding force and high stability, which can further improve the stability of the device.

[0030] 2) In response to the problem of interlayer contact resistance of the device mentioned in the background technology, the present invention in situ grows metal phase nanowires at the micro-interface of the coating through a chemical self-assembly process, and forms a metal nanowire network on the surface and sub-surface of the coating (a certain depth below the surface). The metal layer composed of crossed metal nanowires increases the conductive layer area of ​​the MXene force-sensitive sensing layer. The porous grid structure of the MXene coating is also conducive to forming an electronic barrier, reducing the loss of electrons inside the electrode, thereby further reducing the interface impedance value of the force-sensitive sensing layer, reducing the contact resistance between the interfaces of the flexible device, and improving the detection response sensitivity and signal recognition accuracy.

[0031] 3) The metal nanowires prepared by the chemical self-assembly process can grow and penetrate into the sub-surface layer of the MXene coating to form a network structure, blocking the contact between the MXene sheet and external oxygen and water, avoiding the problem of easy oxidation of MXene mentioned in the background technology to a certain extent, and improving the stability of the device.

[0032] 4) In view of the problems of small sensitive detection range and low mechanical strength of the device mentioned in the background technology, the present invention avoids the problem of self-stacking of MXene sheets due to van der Waals force through microsphere electrostatic self-assembly and thermoforming process, improves the deformation gap and mechanical structure strength of the force-sensitive sensing coating, so that the device can still achieve good sensitivity response when subjected to high-pressure deformation. And the mesh structure of metal nanowires on the coating surface can play a role in distributing stress when subjected to tensile stress.

[0033] 5) The process scheme of the present invention is simple and highly reproducible. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 It is a cross-sectional comparison diagram of the MXene / microsphere coating before and after heat treatment in the process of preparing the sensing layer of the present invention, wherein a is the cross section before treatment and b is the cross section after treatment;

[0035] Figure 2 This is a schematic diagram of the structure of the sensing layer of the present application;

[0036] Figure 3This is a schematic diagram of the preparation of the sensing layer of the present application;

[0037] Figure 4 This is a comparison chart of the water drop contact angle of the PDMS surface after different surface treatment methods of the present application; wherein, a is Example 2-cooperative treatment, b is Comparative Example 1-untreated, c is Comparative Example 2-oxygen plasma cleaning, d is Comparative Example 3-PVA treatment, and e is Comparative Example 4-KH550 treatment;

[0038] Figure 5 This is a graph showing the change of the water drop contact angle on the PDMS surface over time after different surface treatment methods in this application;

[0039] Figure 6 A comparison diagram of the adhesion between the PDMS surface and the sensing layer after different surface treatment methods of the present application;

[0040] Figure 7 This is a sensitivity comparison chart of different functional layer preparation schemes of the present application, wherein Comparative Example 5-single MXene sensing layer (without mesoporous structure and without deposited nanowires), Comparative Example 6-mesoporous structure sensing layer (without deposited nanowires);

[0041] Figure 8 This is a comparison chart of the interface resistance of different functional layer preparation schemes of this application. DETAILED DESCRIPTION

[0042] Example 1

[0043] As shown in the figure, the present invention provides a method for preparing a sensing layer, comprising the following preparation steps:

[0044] S1 handles flexible substrates:

[0045] The PDMS main agent and the hardener were uniformly mixed in a mass ratio of 10:1, and the bubbles in the mixed solution were made to float to the surface and burst by vacuuming to obtain a PDMS mixed solution.

[0046] On the cleaned carrier plate, 2 g of the PDMS mixture was spin-coated at 50 rpm for 2 minutes, and then dried and hardened in a 90°C oven for 2 hours to obtain a PDMS sheet;

[0047] The PDMS sheet was thoroughly degreased in isopropanol, dried with nitrogen, and dehydrated in an oven at 110°C for at least 40 minutes. Then, the PDMS surface was bombarded with inert gas high-energy plasma (nitrogen / argon flow rate of 60 sccm, pressure of 0.67 mbar, power of 300 W, 10 minutes) to create microcracks on the PDMS surface, increase the surface roughness, provide physical sites for subsequent MXene deposition, increase the contact area, and obtain a PDMS flexible substrate.

[0048] The obtained PDMS flexible substrate was cleaned with oxygen plasma (oxygen flow rate of 50 sccm, pressure of 0.67 mbar, power of 100 W, 5 minutes) to hydroxylate the base layer of the PDMS flexible substrate, thereby obtaining a hydroxylated PDMS flexible substrate;

[0049] Prepare PVA solution: Add PVA to pure water and stir at room temperature for 40 minutes. Heat to 100°C and stir for 40 minutes. Finally, stir at 60°C for more than 12 hours, and the mass fraction of PVA solution is 1wt%.

[0050] The hydroxylated PDMS flexible substrate was immersed in the PVA solution for 10 minutes, dried with nitrogen, and heated on a hot plate at 110°C for 15 minutes. The immersion-drying steps were repeated three times to obtain a treated PDMS flexible substrate.

[0051] S2 sensing layer preparation

[0052] Place the treated PDMS flexible substrate on a hot plate at 60°C, and use electrospraying to spray the prepared MXene / microsphere ink onto the treated PDMS flexible substrate surface multiple times. Before each spraying, ensure that the water in the MXene / PS microsphere ink is completely evaporated. Repeated spraying is performed until the MXene / microsphere deposition amount is about 0.2 mg / cm 2 After spraying, the flexible substrate with MXene / PS microsphere coating was placed in a vacuum drying oven at 70°C for 20 minutes, and then the inert gas was pumped in a vacuum sintering furnace several times to exclude oxygen. The vacuum sintering furnace was heated to 350°C at a rate of 100°C / min, and pyrolysis treatment was performed for 13 minutes to make the internal microspheres explode, leaving hollow holes inside, and obtain a flexible substrate with a mesoporous structure MXene film.

[0053] 80 mL of 2.5 mM chloroplatinic acid aqueous solution was mixed with formic acid, and deionized water was added to make the total volume of the mixed solution 100 mL to obtain a platinum ion solution. The flexible substrate of the mesoporous MXene film was placed in the platinum ion solution and allowed to stand for 10 hours. A platinum metal layer was grown on it with the MXene coating as an induction layer. After 72 hours, the electrode sample was washed with deionized water and dried.

[0054] It should be noted that in other embodiments of the present invention, when gold ions need to be deposited on the MXene coating, the flexible substrate on which the MXene coating is deposited can be placed in a solution of an equal volume mixture of 0.01% HAuCl4 solution and 0.4mM hydroxylamine hydrochloride solution, reacted at 18-25°C for 20-30 minutes, taken out and washed with double distilled water, and blown dry with nitrogen. In this way, a gold electrode layer is formed on the MXene coating. When silver ions need to be deposited on the MXene coating, the flexible substrate on which the MXene coating is deposited can be placed in a silver ion solution configured in the following manner: ammonia water is added dropwise to a 10mM silver nitrate solution, the solution turns light brown, ammonia water is continued to be added dropwise until the solution becomes colorless, and then an equal volume of 3.33mM glucose solution is added to the system. The flexible substrate on which the MXene coating is deposited is immersed in the silver ion solution, reacted at 18-25°C for 2-10 minutes, taken out and washed with double distilled water, and blown dry with nitrogen, so that a silver electrode layer is formed on the MXene coating. When copper ions need to be deposited on the MXene coating, the flexible substrate on which the MXene coating is deposited can be placed in a copper ion solution prepared in the following manner: prepare a solution containing 50mM EDTA, 50mM CuCl2 and 0.1M H3BO3, adjust the pH to 7, and then add a volume of 0.1M dimethylamine borane solution to obtain a mixed solution. The flexible substrate on which the MXene coating is deposited is immersed in the copper ion solution, reacted at 40°C with nitrogen for 2 hours, and then taken out and washed with double distilled water and dried with nitrogen, so that a copper electrode layer is formed on the MXene coating.

[0055] The present invention provides a sensor, comprising a sensor layer made by the above-mentioned method for preparing a sensor layer. The preparation steps include:

[0056] S1 Preparation of microsphere dispersion: The prepared microsphere solution is dispersed in a cationic polymer polydiallyldimethylammonium chloride (PDDA) solution (0.1 wt%) by ultrasonic treatment. After vigorous stirring for 12 hours, the mixture is filtered with a 0.22 μm aqueous filter membrane, and washed with deionized water for several times to remove excess PDDA, and the microspheres on the aqueous filter membrane are dispersed again in deionized water to obtain a positively charged microsphere dispersion;

[0057] Preparation of single-layer MXene solution: multilayer MXene powder was dissolved in water, and ultrasonicated for 30 minutes under the protection of inert gas to destroy the multilayer structure. During this period, the water temperature was controlled below 40°C by ice bath and other means to avoid MXene oxidation, and a MXene dispersion was obtained.

[0058] The MXene dispersion obtained by ultrasound was centrifuged at a high speed of more than 5000 rpm for 10 minutes, and the supernatant was the single-layer MXene solution.

[0059] The concentration of the monolayer MXene solution was determined by vacuum filtration of the film and adjusted to 1 mg / ml.

[0060] The microsphere dispersion was added dropwise to the monolayer MXene solution for electrostatic self-assembly. The mass ratio of microspheres to MXene should be 1:2. The MXene / microsphere dispersion was slowly stirred for 20 minutes. During the stirring process, the negatively charged MXene nanosheets were spontaneously wrapped on the surface of the PS microspheres through electrostatic self-assembly. The prepared MXene / PS microsphere ink was further concentrated by high-speed centrifugation (6000 rpm, 20 minutes); the average diameter of the microspheres should be controlled at 0.5-2 microns.

[0061] S2 prepares the sensing layer;

[0062] S3 flexible electrode film preparation

[0063] The flexible film is used as a substrate, and the obtained flexible substrate is evenly sprayed with photoresist. The flexible film with photoresist is dried on a constant temperature heating table at 80°C for 30 minutes to cure the photoresist.

[0064] Using an inkjet printer to print a desired interdigital electrode pattern on a film as a mask;

[0065] Place the pattern surface of the mask close to the cured photoresist coating, expose to ultraviolet light for 3 minutes, and use a developer to soak and remove the photoresist on the patterned part;

[0066] After the sample was plasma cleaned with argon and oxygen, titanium layer, copper layer, and gold layer were magnetron sputtered on the surface in sequence;

[0067] The remaining photoresist and the metal layer thereon are removed by a release agent to obtain a patterned interdigital electrode layer.

[0068] The flexible film is made of a flexible insulating material, polyimide (PI), which has good bending resistance and insulation properties.

[0069] S4 Assembly

[0070] Use copper wire to connect the two electrodes of the interdigital electrode through conductive silver paste to establish an external circuit. Coat PDMS on the top layer as a fixative, treat the flexible substrate and the sensing layer and flexible electrode film obtained in the above steps with oxygen plasma, and vertically plane-laminate in the order of encapsulation layer-electrode layer-sensing layer-flexible substrate-encapsulation layer. Use the flexible film as the encapsulation layer to assemble the above components into a flexible sensor.

[0071] The material of the flexible film is a flexible insulating material, which can be selected from one or more of polyimide (PI), polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polymethyl methacrylate (PMMA) and polyurethane (PUA), and the microspheres can be selected from one or more of polystyrene (PS) microspheres, polymethyl methacrylate (PMMA) microspheres, polystyrene-co-acrylate (PS-b-PMMA) copolymer microspheres, and polylactic acid (PLA) microspheres.

[0072] The time for which the flexible substrate on which the MXene coating is deposited is placed in the solution of metal ions can be determined according to the specific metal ions and their concentrations. For example, when growing a platinum metal electrode layer, the placement time can be 10 hours; when growing a copper metal electrode layer, the placement time can be 1-5 hours.

[0073] Example 2

[0074] The present invention provides a method for preparing a sensing layer, comprising the following preparation steps:

[0075] S1 handles flexible substrates:

[0076] The PDMS main agent and the hardener are evenly mixed in a mass ratio of 9:1, and the bubbles in the mixed solution are floated to the surface and burst by vacuuming to obtain a PDMS mixed solution;

[0077] On the cleaned carrier plate, 3 g of the PDMS mixture was spin-coated at 40 rpm for 5 minutes, and then dried and hardened in a 90°C oven for 5 hours to obtain a PDMS sheet;

[0078] The PDMS sheet was thoroughly degreased in isopropanol, dried with nitrogen, and dehydrated in an oven at 110°C for at least 40 minutes. The PDMS surface was then bombarded with inert gas high-energy plasma (nitrogen / argon flow rate of 70 sccm, pressure of 0.6 mbar, power of 400 W, for 12 minutes) to create microcracks on the PDMS surface, increase the surface roughness, provide physical sites for subsequent MXene deposition, increase the contact area, and obtain a PDMS flexible substrate.

[0079] The obtained PDMS flexible substrate was cleaned by oxygen plasma (oxygen flow rate of 100 sccm, pressure of 0.8 mbar, power of 100 W, 7 minutes) to hydroxylate the base layer of the PDMS flexible substrate, thereby obtaining a hydroxylated PDMS flexible substrate;

[0080] Prepare PVA solution: Add PVA to pure water and stir at room temperature for 50 minutes. Heat to 120°C and stir for 50 minutes. Finally, stir at 70°C for more than 12 hours. The mass fraction of PVA solution is 0.5wt%.

[0081] The hydroxylated PDMS flexible substrate was immersed in the PVA solution for 13 minutes, dried with nitrogen, and heated on a hot plate at 120° C. for 20 minutes. The immersion-drying steps were repeated three times to obtain a treated PDMS flexible substrate.

[0082] S2 sensing layer preparation

[0083] Place the treated PDMS flexible substrate on a hot plate at 60°C, and use electrospraying to spray the prepared MXene / microsphere ink onto the treated PDMS flexible substrate surface multiple times. Before each spraying, ensure that the water in the MXene / PMMA microsphere ink is completely evaporated. Repeated spraying is performed until the MXene / PMMA microsphere deposition amount is about 0.3 mg / cm 2 After spraying, the flexible substrate with MXene / PMMA microsphere coating is placed in a vacuum drying oven at 60°C for 25 minutes to remove interlayer water, and then placed in a high-temperature vacuum sintering furnace. Under the protection of inert gas, it is pyrolyzed at 500°C for 20 minutes to make the microspheres inside the coating burst, leaving hollow holes inside; a flexible substrate of mesoporous MXene film is obtained. Before high-temperature pyrolysis, the high-temperature furnace should be filled with inert gas several times to exclude oxygen; the heating temperature of the high-temperature furnace should be controlled at more than 100°C / minute to prevent the microspheres from slowly melting due to heat.

[0084] The flexible substrate of the mesoporous MXene film was placed in a solution of equal volumes of 0.01% HAuCl4 solution and 0.4mM hydroxylamine hydrochloride solution, and reacted at 18-25°C for 20-30 minutes. The substrate was taken out and washed with double distilled water and dried with nitrogen to form a gold electrode layer on the MXene coating. After 72 hours, the electrode sample was washed with deionized water and dried.

[0085] The present invention provides a sensor, comprising a sensor layer made by the above-mentioned method for preparing a sensor layer. The preparation steps include:

[0086] S1 Preparation of microsphere dispersion: The prepared microsphere solution is dispersed in a cationic polymer polydiallyldimethylammonium chloride (PDDA) solution (0.1 wt%) by ultrasonic treatment. After vigorous stirring for 12 hours, the mixture is filtered with a 0.22 μm aqueous filter membrane, and washed with deionized water for several times to remove excess PDDA, and the microspheres on the aqueous filter membrane are dispersed again in deionized water to obtain a positively charged microsphere dispersion;

[0087] Preparation of single-layer MXene solution: multilayer MXene powder was dissolved in water, and ultrasonicated for 40 minutes under the protection of inert gas to destroy the multilayer structure. During this period, the water temperature was controlled below 40°C by ice bath and other means to avoid MXene oxidation, and a MXene dispersion was obtained.

[0088] The MXene dispersion obtained by ultrasound was centrifuged at a high speed of more than 5000 rpm for 10 minutes, and the supernatant was the single-layer MXene solution.

[0089] The concentration of the monolayer MXene solution was determined by vacuum filtration of the film and adjusted to 1 mg / ml.

[0090] The microsphere dispersion was added dropwise to the monolayer MXene solution for electrostatic self-assembly. The mass ratio of PMMA microspheres to MXene should be 1:2. The MXene / PMMA microsphere dispersion was slowly stirred for 20 minutes. During the stirring process, the negatively charged MXene nanosheets were spontaneously wrapped on the surface of the PMMA microspheres through electrostatic self-assembly. The prepared MXene / PMMA microsphere ink was further concentrated using high-speed centrifugation (6000 rpm, 20 minutes); the average diameter of the microspheres should be controlled at 0.5-2 microns.

[0091] S2 prepares the sensing layer;

[0092] S3 flexible electrode film preparation

[0093] The flexible film is used as a substrate, and the obtained flexible substrate is evenly sprayed with photoresist. The flexible film with photoresist is dried on a constant temperature heating table at 80°C for 30 minutes to cure the photoresist.

[0094] Using an inkjet printer to print a desired interdigital electrode pattern on a film as a mask;

[0095] Place the pattern surface of the mask close to the cured photoresist coating, expose to ultraviolet light for 3 minutes, and use a developer to soak and remove the photoresist on the patterned part;

[0096] After the sample was plasma cleaned with argon and oxygen, titanium layer, copper layer, and gold layer were magnetron sputtered on the surface in sequence;

[0097] The remaining photoresist and the metal layer thereon are removed by a release agent to obtain a patterned interdigital electrode layer.

[0098] Wherein, the material of the flexible film is polyethylene terephthalate (PET)

[0099] S4 Assembly

[0100] Use copper wire to connect the two electrodes of the interdigital electrode through conductive silver paste to establish an external circuit. Coat PDMS on the top layer as a fixative, treat the flexible substrate and the sensing layer and flexible electrode film obtained in the above steps with oxygen plasma, and vertically plane-laminate in the order of encapsulation layer-electrode layer-sensing layer-flexible substrate-encapsulation layer. Use the flexible film as the encapsulation layer to assemble the above components into a flexible sensor.

[0101] Example 3

[0102] The present invention provides a method for preparing a sensing layer, comprising the following preparation steps:

[0103] S1 handles flexible substrates:

[0104] The PDMS main agent and the hardener are evenly mixed in a mass ratio of 11:1, and the bubbles in the mixed solution are floated to the surface and burst by vacuuming to obtain a PDMS mixed solution;

[0105] On the cleaned carrier plate, 2 g of the PDMS mixture was spin-coated at 60 rpm for 1 minute, and then dried and hardened in a 90°C oven for 1 hour to obtain a PDMS sheet;

[0106] The PDMS sheet was thoroughly degreased in isopropanol, dried with nitrogen, and dehydrated in an oven at 110°C for at least 40 minutes. Then, the PDMS surface was bombarded with inert gas high-energy plasma (nitrogen / argon flow rate of 50 sccm, pressure of 0.8 mbar, power of 400 W, 8 minutes) to create microcracks on the PDMS surface, increase the surface roughness, provide physical sites for subsequent MXene deposition, increase the contact area, and obtain a PDMS flexible substrate.

[0107] The obtained PDMS flexible substrate was cleaned with oxygen plasma (oxygen flow rate of 30 sccm, pressure of 0.6 mbar, power of 100 W, 1 minute) to hydroxylate the base layer of the PDMS flexible substrate, thereby obtaining a hydroxylated PDMS flexible substrate;

[0108] Prepare PVA solution: Add PVA to pure water and stir at room temperature for 30 minutes. Heat to 90°C and stir for 30 minutes. Finally, stir at 50°C for more than 12 hours. The mass fraction of PVA solution is 2wt%.

[0109] The hydroxylated PDMS flexible substrate was immersed in the PVA solution for 8 minutes, dried with nitrogen, and heated on a hot plate at 100° C. for 10 minutes. The immersion-drying steps were repeated three times to obtain a treated PDMS flexible substrate.

[0110] S2 sensing layer preparation

[0111] Place the treated PDMS flexible substrate on a hot plate at 60°C, and use electrospraying to spray the prepared MXene / PLA microsphere ink onto the treated PDMS flexible substrate surface multiple times. Before each spraying, ensure that the water in the MXene / PLA microsphere dispersion is completely evaporated. Repeated spraying is performed until the MXene / PLA microsphere deposition amount is about 0.1 mg / cm 2After spraying, the flexible substrate with MXene / PLA microsphere coating is placed in a vacuum drying oven at 70°C for 20 minutes to remove interlayer water, and then placed in a high-temperature vacuum sintering furnace. Under the protection of inert gas, it is pyrolyzed at 350°C for 13 minutes to make the microspheres inside the coating burst, leaving hollow holes inside; a flexible substrate with a mesoporous structure MXene film is obtained. Before high-temperature pyrolysis, the high-temperature furnace should be filled with inert gas several times to exclude oxygen; the heating temperature of the high-temperature furnace should be controlled at above 100°C / minute to prevent the microspheres from slowly melting due to heat.

[0112] Ammonia water was added to a 10mM silver nitrate solution, and the solution turned light brown. Ammonia water was added until the solution turned colorless, and then an equal volume of 3.33mM glucose solution was added to the system. The flexible substrate of the mesoporous MXene film was immersed in the silver ion solution, reacted at 18-25°C for 2-10 minutes, taken out and washed with double distilled water, dried with nitrogen, and a silver electrode layer was formed on the MXene coating. After 48 hours, the electrode sample was washed with deionized water and dried.

[0113] When copper ions need to be deposited on the MXene coating, the flexible substrate on which the MXene coating is deposited can be placed in a copper ion solution prepared in the following manner: prepare a solution containing 50mM EDTA, 50mM CuCl2 and 0.1M H3BO3, adjust the pH to 7, and then add a volume of 0.1M dimethylamine borane solution to obtain a mixed solution. The flexible substrate on which the MXene coating is deposited is immersed in the copper ion solution, reacted at 40°C with nitrogen for 2 hours, and then taken out and washed with double distilled water and dried with nitrogen, so that a copper electrode layer is formed on the MXene coating.

[0114] The present invention provides a sensor, comprising a sensor layer made by the above-mentioned method for preparing a sensor layer. The preparation steps include:

[0115] S1 Preparation of microsphere dispersion: The prepared PLA microsphere solution is dispersed in a cationic polymer polydiallyldimethylammonium chloride (PDDA) solution (0.1 wt%) by ultrasonic treatment. After vigorous stirring for 12 hours, the mixture is filtered with a 0.22 μm aqueous filter membrane and washed with deionized water for several times to remove excess PDDA, and the microspheres on the aqueous filter membrane are dispersed again in deionized water to obtain a positively charged microsphere dispersion;

[0116] Preparation of single-layer MXene solution: multilayer MXene powder was dissolved in water, and ultrasonicated for 20 minutes under the protection of inert gas to destroy the multilayer structure. During this period, the water temperature was controlled below 40°C by ice bath and other means to avoid MXene oxidation, and a MXene dispersion was obtained.

[0117] The MXene dispersion obtained by ultrasound was centrifuged at a high speed of more than 5000 rpm for 10 minutes, and the supernatant was the single-layer MXene solution.

[0118] The concentration of the monolayer MXene solution was determined by vacuum filtration of the film and adjusted to 1 mg / ml.

[0119] The microsphere dispersion was added dropwise to the monolayer MXene solution for electrostatic self-assembly. The mass ratio of microspheres to MXene should be 1:2. The MXene / PLA microsphere dispersion was slowly stirred for 20 minutes. During the stirring process, the negatively charged MXene nanosheets were spontaneously wrapped on the surface of the PLA microspheres through electrostatic self-assembly. The prepared MXene / PLAS microsphere ink was further concentrated by high-speed centrifugation (6000 rpm, 20 minutes); the average diameter of the microspheres should be controlled at 0.5-2 microns.

[0120] S2 prepares the sensing layer;

[0121] S3 flexible electrode film preparation

[0122] The flexible film is used as a substrate, the obtained flexible substrate is evenly sprayed with photoresist, and the flexible film with photoresist is dried on a constant temperature heating table at 80° C. for 30 minutes to solidify the photoresist;

[0123] Using an inkjet printer to print a desired interdigital electrode pattern on a film as a mask;

[0124] Place the pattern surface of the mask close to the cured photoresist coating, expose to ultraviolet light for 3 minutes, and use a developer to soak and remove the photoresist on the patterned part;

[0125] After the sample was plasma cleaned with argon and oxygen, titanium layer, copper layer, and gold layer were magnetron sputtered on the surface in sequence;

[0126] The remaining photoresist and the metal layer thereon are removed by a release agent to obtain a patterned interdigital electrode layer.

[0127] Wherein, the material of the flexible film is polyethylene naphthalate (PEN)

[0128] S4 Assembly

[0129] Use copper wire to connect the two electrodes of the interdigital electrode through conductive silver paste to establish an external circuit. Coat PDMS on the top layer as a fixative, treat the flexible substrate and the sensing layer and flexible electrode film obtained in the above steps with oxygen plasma, and vertically plane-laminate in the order of encapsulation layer-electrode layer-sensing layer-flexible substrate-encapsulation layer. Use the flexible film as the encapsulation layer to assemble the above components into a flexible sensor.

[0130] Comparative Example 1

[0131] The PDMS surface of this comparative example 1 was not treated, and the remaining steps were the same as those of example 2.

[0132] This comparative example provides a method for preparing a sensing layer, comprising the following preparation steps:

[0133] S1 handles flexible substrates:

[0134] The PDMS main agent and the hardener are evenly mixed in a mass ratio of 9:1, and the bubbles in the mixed solution are floated to the surface and burst by vacuuming to obtain a PDMS mixed solution;

[0135] On the cleaned carrier plate, 3 g of the PDMS mixture was spin-coated at 40 rpm for 5 minutes, and then dried and hardened in a 90°C oven for 5 hours to obtain a PDMS sheet;

[0136] The PDMS sheet was thoroughly degreased in isopropanol, blown dry with nitrogen, and dehydrated in an oven at 110 °C for at least 40 min to obtain a PDMS flexible substrate.

[0137] S2 sensing layer preparation

[0138] Place the PDMS flexible substrate on a hot plate at 60°C, and use electrospraying to spray the prepared MXene / microsphere ink onto the treated PDMS flexible substrate surface multiple times. Before each spraying, ensure that the water in the MXene / PMMA microsphere dispersion is completely evaporated. Repeated spraying is performed until the MXene / PMMA microsphere deposition amount is about 0.3 mg / cm 2 After spraying, the flexible substrate with MXene / PMMA microsphere coating is placed in a vacuum drying oven at 60°C for 25 minutes to remove interlayer water, and then placed in a high-temperature vacuum sintering furnace. Under the protection of inert gas, it is pyrolyzed at 500°C for 20 minutes to make the microspheres inside the coating burst, leaving hollow holes inside; a flexible substrate of mesoporous MXene film is obtained. Before high-temperature pyrolysis, the high-temperature furnace should be filled with inert gas several times to exclude oxygen; the heating temperature of the high-temperature furnace should be controlled at more than 100°C / minute to prevent the microspheres from slowly melting due to heat.

[0139] The flexible substrate of the obtained mesoporous MXene film was placed in a solution of equal volumes of 0.01% HAuCl4 solution and 0.4mM hydroxylamine hydrochloride solution, reacted at 18-25°C for 20-30 minutes, taken out and washed with double distilled water, and blown dry with nitrogen to form a gold electrode layer on the MXene coating. After 72 hours, the electrode sample was washed with deionized water and dried.

[0140] This comparative example provides a sensor, including a sensor layer prepared by the above-mentioned method for preparing a sensor layer, including the following preparation steps:

[0141] S1 Preparation of microsphere dispersion: The prepared microsphere solution is dispersed in a cationic polymer polydiallyldimethylammonium chloride (PDDA) solution (0.1 wt%) by ultrasonic treatment. After vigorous stirring for 12 hours, the mixture is filtered with a 0.22 μm aqueous filter membrane, and washed with deionized water for several times to remove excess PDDA, and the microspheres on the aqueous filter membrane are dispersed again in deionized water to obtain a positively charged microsphere dispersion;

[0142] Preparation of single-layer MXene solution: multilayer MXene powder was dissolved in water, and ultrasonicated for 40 minutes under the protection of inert gas to destroy the multilayer structure. During this period, the water temperature was controlled below 40°C by ice bath and other means to avoid MXene oxidation, and a MXene dispersion was obtained.

[0143] The MXene dispersion obtained by ultrasound was centrifuged at a high speed of more than 5000 rpm for 10 minutes, and the supernatant was the single-layer MXene solution.

[0144] The concentration of the monolayer MXene solution was determined by vacuum filtration of the film and adjusted to 1 mg / ml.

[0145] The microsphere dispersion was added dropwise to the monolayer MXene solution for electrostatic self-assembly. The mass ratio of PMMA microspheres to MXene should be 1:2. The MXene / PMMA microsphere dispersion was slowly stirred for 20 minutes. During the stirring process, the negatively charged MXene nanosheets were spontaneously wrapped on the surface of the PMMA microspheres through electrostatic self-assembly. The prepared MXene / PMMA microsphere ink was further concentrated using high-speed centrifugation (6000 rpm, 20 minutes); the average diameter of the microspheres should be controlled at 0.5-2 microns.

[0146] S2 prepares the sensing layer;

[0147] S3 flexible electrode film preparation

[0148] The flexible film is used as a substrate, and the obtained flexible substrate is evenly sprayed with photoresist. The flexible film with photoresist is dried on a constant temperature heating table at 80°C for 30 minutes to cure the photoresist.

[0149] Using an inkjet printer to print a desired interdigital electrode pattern on a film as a mask;

[0150] Place the pattern surface of the mask close to the cured photoresist coating, expose to ultraviolet light for 3 minutes, and use a developer to soak and remove the photoresist on the patterned part;

[0151] After the sample was plasma cleaned with argon and oxygen, titanium layer, copper layer, and gold layer were magnetron sputtered on the surface in sequence;

[0152] The remaining photoresist and the metal layer thereon are removed by a release agent to obtain a patterned interdigital electrode layer.

[0153] Wherein, the material of the flexible film is polyethylene terephthalate (PET)

[0154] S4 Assembly

[0155] Use copper wire to connect the two electrodes of the interdigital electrode through conductive silver paste to establish an external circuit. Coat PDMS on the top layer as a fixative, treat the flexible substrate and the sensing layer and flexible electrode film obtained in the above steps with oxygen plasma, and vertically plane-laminate in the order of encapsulation layer-electrode layer-sensing layer-flexible substrate-encapsulation layer. Use the flexible film as the encapsulation layer to assemble the above components into a flexible sensor.

[0156] Comparative Example 2

[0157] In this comparative example, the PDMS surface is only subjected to high-energy plasma treatment, and the remaining steps and parameters are the same as those in Example 2. This comparative example provides a method for preparing a sensing layer, comprising the following preparation steps:

[0158] S1 handles flexible substrates:

[0159] The PDMS main agent and the hardener are uniformly mixed in a mass ratio of 9:1, and the bubbles in the mixed solution are floated to the surface and burst by vacuuming to obtain a PDMS mixed solution;

[0160] On the cleaned carrier plate, 3 g of the PDMS mixture was spin-coated at 40 rpm for 5 minutes, and then dried and hardened in a 90° C. oven for 5 hours to obtain a PDMS sheet;

[0161] The PDMS sheet was thoroughly degreased in isopropanol, dried with nitrogen, and dehydrated in an oven at 110 °C for at least 40 min, and oxygen plasma cleaned (oxygen flow rate of 10 sccm, pressure of 0.8 mbar, power of 100 W, 7 min) to obtain a hydroxylated PDMS flexible substrate;

[0162] Prepare PVA solution: Add PVA to pure water and stir at room temperature for 50 minutes. Heat to 120°C and stir for 50 minutes. Finally, stir at 70°C for more than 12 hours. The mass fraction of PVA solution is 0.5wt%.

[0163] The hydroxylated PDMS flexible substrate was immersed in the PVA solution for 13 minutes, dried with nitrogen, and heated on a hot plate at 120° C. for 20 minutes. The immersion-drying steps were repeated three times to obtain a treated PDMS flexible substrate.

[0164] S2 sensing layer preparation

[0165] Place the treated PDMS flexible substrate on a hot plate at 60°C, and use electrospraying to spray the prepared MXene / microsphere dispersion onto the surface of the PDMS flexible substrate multiple times. Before each spraying, ensure that the water in the MXene / PMMA microsphere dispersion is completely evaporated. Repeated spraying is performed until the MXene / PMMA microsphere deposition amount is about 0.3 mg / cm 2 After spraying, the flexible substrate with MXene / PMMA microsphere coating is placed in a vacuum drying oven at 60°C for 25 minutes to remove interlayer water, and then placed in a high-temperature vacuum sintering furnace. Under the protection of inert gas, it is pyrolyzed at 500°C for 20 minutes to make the microspheres inside the coating burst, leaving hollow holes inside; a flexible substrate of mesoporous MXene film is obtained. Before high-temperature pyrolysis, the high-temperature furnace should be filled with inert gas several times to exclude oxygen; the heating temperature of the high-temperature furnace should be controlled at more than 100°C / minute to prevent the microspheres from slowly melting due to heat.

[0166] The flexible substrate of the obtained mesoporous MXene film was placed in a solution of equal volumes of 0.01% HAuCl4 solution and 0.4mM hydroxylamine hydrochloride solution, and reacted at 18-25°C for 20-30 minutes. The substrate was taken out and washed with double distilled water and dried with nitrogen to form a gold electrode layer on the MXene coating. After 72 hours, the electrode sample was washed with deionized water and dried.

[0167] The present invention provides a sensor, comprising a sensor layer made by the above-mentioned method for preparing a sensor layer. The preparation steps include:

[0168] S1 Preparation of microsphere dispersion: The prepared microsphere solution is dispersed in a cationic polymer polydiallyldimethylammonium chloride (PDDA) solution (0.1 wt%) by ultrasonic treatment. After vigorous stirring for 12 hours, the mixture is filtered with a 0.22 μm aqueous filter membrane, and washed with deionized water for several times to remove excess PDDA, and the microspheres on the aqueous filter membrane are dispersed again in deionized water to obtain a positively charged microsphere dispersion;

[0169] Preparation of single-layer MXene solution: Dissolve multilayer MXene powder in water, and under the protection of inert gas, ultrasonicate for 40 minutes to destroy the multilayer structure. During this period, control the water temperature below 40°C by ice bath or other means to avoid MXene oxidation.

[0170] The MXene dispersion obtained by ultrasound was centrifuged at a high speed of more than 5000 rpm for 10 minutes, and the supernatant was the single-layer MXene solution.

[0171] The concentration of the monolayer MXene solution was determined by vacuum filtration of the film and adjusted to 1 mg / ml.

[0172] The microsphere dispersion was added dropwise to the monolayer MXene solution for electrostatic self-assembly. The mass ratio of PMMA microspheres to MXene should be 1:2. The MXene / PMMA microsphere dispersion was slowly stirred for 20 minutes. During the stirring process, the negatively charged MXene nanosheets were spontaneously wrapped on the surface of the PMMA microspheres through electrostatic self-assembly. The prepared MXene / PMMA microsphere ink was further concentrated using high-speed centrifugation (6000 rpm, 20 minutes); the average diameter of the microspheres should be controlled at 0.5-2 microns.

[0173] S2 prepares the sensing layer;

[0174] S3 flexible electrode film preparation

[0175] The flexible film is used as a substrate, and the obtained flexible substrate is evenly sprayed with photoresist. The flexible film with photoresist is dried on a constant temperature heating table at 80°C for 30 minutes to cure the photoresist.

[0176] Using an inkjet printer to print a desired interdigital electrode pattern on a film as a mask;

[0177] Place the pattern surface of the mask close to the cured photoresist coating, expose to ultraviolet light for 3 minutes, and use a developer to soak and remove the photoresist on the patterned part;

[0178] After the sample was plasma cleaned with argon and oxygen, titanium layer, copper layer, and gold layer were magnetron sputtered on the surface in sequence;

[0179] The remaining photoresist and the metal layer thereon are removed by a release agent to obtain a patterned interdigital electrode layer.

[0180] Wherein, the material of the flexible film is polyethylene terephthalate (PET)

[0181] S4 Assembly

[0182] Use copper wire to connect the two electrodes of the interdigital electrode through conductive silver paste to establish an external circuit. Coat PDMS on the top layer as a fixative, treat the flexible substrate and the sensing layer and flexible electrode film obtained in the above steps with oxygen plasma, and vertically plane-laminate in the order of encapsulation layer-electrode layer-sensing layer-flexible substrate-encapsulation layer. Use the flexible film as the encapsulation layer to assemble the above components into a flexible sensor.

[0183] Comparative Example 3

[0184] In this comparative example, the PDMS surface was only modified by chemical grafting of PVA, and the remaining steps and parameters were the same as those in Example 2.

[0185] This comparative example provides a method for preparing a sensing layer, comprising the following preparation steps:

[0186] S1 handles flexible substrates:

[0187] The PDMS main agent and the hardener are uniformly mixed in a mass ratio of 9:1, and the bubbles in the mixed solution are floated to the surface and burst by vacuuming to obtain a PDMS mixed solution;

[0188] On the cleaned carrier plate, 3 g of the PDMS mixture was spin-coated at 40 rpm for 5 minutes, and then dried and hardened in a 90° C. oven for 5 hours to obtain a PDMS sheet;

[0189] The PDMS sheet was thoroughly degreased in isopropanol, dried with nitrogen, and dehydrated in an oven at 110 °C for at least 40 min to obtain a PDMS flexible substrate;

[0190] Prepare PVA solution: Add PVA to pure water and stir at room temperature for 50 minutes. Heat to 120°C and stir for 50 minutes. Finally, stir at 70°C for more than 12 hours. The mass fraction of PVA solution is 0.5wt%.

[0191] The hydroxylated PDMS flexible substrate was immersed in the PVA solution for 13 minutes, dried with nitrogen, and heated on a hot plate at 120° C. for 20 minutes. The immersion-drying steps were repeated three times to obtain a treated PDMS flexible substrate.

[0192] S2 sensing layer preparation

[0193] Place the treated PDMS flexible substrate on a hot plate at 60°C, and use electrospraying to spray the prepared MXene / microsphere dispersion onto the surface of the PDMS flexible substrate multiple times. Before each spraying, ensure that the water in the MXene / PMMA microsphere dispersion is completely evaporated. Repeated spraying is performed until the MXene / PMMA microsphere deposition amount is about 0.3 mg / cm 2 After spraying, the flexible substrate with MXene / PMMA microsphere coating is placed in a vacuum drying oven at 60°C for 25 minutes to remove interlayer water, and then placed in a high-temperature vacuum sintering furnace. Under the protection of inert gas, pyrolysis treatment is performed at 500°C for 20 minutes to make the microspheres inside the coating burst, leaving hollow holes inside; a flexible substrate with a mesoporous MXene film is obtained. Before high-temperature pyrolysis, the high-temperature furnace should be filled with inert gas several times to exclude oxygen; the heating temperature of the high-temperature furnace should be controlled at above 100°C / minute to prevent the microspheres from slowly melting due to heat.

[0194] The flexible substrate of the obtained mesoporous MXene film was placed in a solution of equal volumes of 0.01% HAuCl4 solution and 0.4mM hydroxylamine hydrochloride solution, and reacted at 18-25°C for 20-30 minutes. The substrate was taken out and washed with double distilled water and dried with nitrogen to form a gold electrode layer on the MXene coating. After 72 hours, the electrode sample was washed with deionized water and dried.

[0195] The present invention provides a sensor, comprising a sensor layer made by the above-mentioned method for preparing a sensor layer. The preparation steps include:

[0196] S1 Preparation of microsphere dispersion: The prepared microsphere solution is dispersed in a cationic polymer polydiallyldimethylammonium chloride (PDDA) solution (0.1 wt%) by ultrasonic treatment. After vigorous stirring for 12 hours, the mixture is filtered with a 0.22 μm aqueous filter membrane, and washed with deionized water for several times to remove excess PDDA, and the microspheres on the aqueous filter membrane are dispersed again in deionized water to obtain a positively charged microsphere dispersion;

[0197] Preparation of single-layer MXene solution: Dissolve multilayer MXene powder in water, and under the protection of inert gas, ultrasonicate for 40 minutes to destroy the multilayer structure. During this period, control the water temperature below 40°C by ice bath or other means to avoid MXene oxidation.

[0198] The MXene dispersion obtained by ultrasound was centrifuged at a high speed of more than 5000 rpm for 10 minutes, and the supernatant was the single-layer MXene solution.

[0199] The concentration of the monolayer MXene solution was determined by vacuum filtration of the film and adjusted to 1 mg / ml.

[0200] The microsphere dispersion was added dropwise to the monolayer MXene solution for electrostatic self-assembly. The mass ratio of PMMA microspheres to MXene should be 1:2. The MXene / PMMA microsphere dispersion was slowly stirred for 20 minutes. During the stirring process, the negatively charged MXene nanosheets were spontaneously wrapped on the surface of the PMMA microspheres through electrostatic self-assembly. The prepared MXene / PMMA microsphere ink was further concentrated using high-speed centrifugation (6000 rpm, 20 minutes); the average diameter of the microspheres should be controlled at 0.5-2 microns.

[0201] S2 prepares the sensing layer;

[0202] S3 flexible electrode film preparation

[0203] The flexible film is used as a substrate, and the obtained flexible substrate is evenly sprayed with photoresist. The flexible film with photoresist is dried on a constant temperature heating table at 80°C for 30 minutes to cure the photoresist.

[0204] Using an inkjet printer to print a desired interdigital electrode pattern on a film as a mask;

[0205] Place the pattern surface of the mask close to the cured photoresist coating, expose to ultraviolet light for 3 minutes, and use a developer to soak and remove the photoresist on the patterned part;

[0206] After the sample was plasma cleaned with argon and oxygen, titanium layer, copper layer, and gold layer were magnetron sputtered on the surface in sequence;

[0207] The remaining photoresist and the metal layer thereon are removed by a release agent to obtain a patterned interdigital electrode layer.

[0208] Wherein, the material of the flexible film is polyethylene terephthalate (PET)

[0209] S4 Assembly

[0210] Use copper wire to connect the two electrodes of the interdigital electrode through conductive silver paste to establish an external circuit. Coat PDMS on the top layer as a fixative, treat the flexible substrate and the sensing layer and flexible electrode film obtained in the above steps with oxygen plasma, and vertically plane-laminate in the order of encapsulation layer-electrode layer-sensing layer-flexible substrate-encapsulation layer. Use the flexible film as the encapsulation layer to assemble the above components into a flexible sensor.

[0211] Comparative Example 4

[0212] In this comparative example, the PDMS surface was only treated with KH550, and the remaining steps and parameters were the same as those in Example 2.

[0213] The preparation method of the sensing layer of this comparative example includes the following preparation steps:

[0214] S1 handles flexible substrates:

[0215] The PDMS main agent and the hardener are uniformly mixed in a mass ratio of 9:1, and the bubbles in the mixed solution are floated to the surface and burst by vacuuming to obtain a PDMS mixed solution;

[0216] On the cleaned carrier plate, 3 g of the PDMS mixture was spin-coated at 40 rpm for 5 minutes, and then dried and hardened in a 90° C. oven for 5 hours to obtain a PDMS sheet;

[0217] The PDMS sheet was thoroughly degreased in isopropanol, dried with nitrogen, and dehydrated in an oven at 110 °C for at least 40 min to obtain a PDMS flexible substrate.

[0218] The PDMS flexible substrate was immersed in the KH550 solution for 5 minutes, taken out and dried with nitrogen, and heated on a hot plate at 120° C. for 20 minutes. The immersion-drying steps were repeated three times to obtain a treated PDMS flexible substrate.

[0219] S2 sensing layer preparation

[0220] Place the treated PDMS flexible substrate on a hot plate at 60°C, and use electrospraying to spray the prepared MXene / microsphere dispersion onto the surface of the PDMS flexible substrate multiple times. Before each spraying, ensure that the water in the MXene / PMMA microsphere dispersion is completely evaporated. Repeated spraying is performed until the MXene / PMMA microsphere deposition amount is about 0.3 mg / cm 2 After spraying, the flexible substrate with MXene / PMMA microsphere coating is placed in a vacuum drying oven at 60°C for 25 minutes to remove interlayer water, and then placed in a high-temperature vacuum sintering furnace. Under the protection of inert gas, it is pyrolyzed at 500°C for 20 minutes to make the microspheres inside the coating burst, leaving hollow holes inside; a flexible substrate of mesoporous MXene film is obtained. Before high-temperature pyrolysis, the high-temperature furnace should be filled with inert gas several times to exclude oxygen; the heating temperature of the high-temperature furnace should be controlled at more than 100°C / minute to prevent the microspheres from slowly melting due to heat.

[0221] The flexible substrate of the obtained mesoporous MXene film was placed in a solution of equal volumes of 0.01% HAuCl4 solution and 0.4mM hydroxylamine hydrochloride solution, and reacted at 18-25°C for 20-30 minutes. The substrate was taken out and washed with double distilled water and dried with nitrogen to form a gold electrode layer on the MXene coating. After 72 hours, the electrode sample was washed with deionized water and dried.

[0222] The sensor of this comparative example comprises the following preparation steps:

[0223] S1 Preparation of microsphere dispersion: The prepared microsphere solution is dispersed in a cationic polymer polydiallyldimethylammonium chloride (PDDA) solution (0.1 wt%) by ultrasonic treatment. After vigorous stirring for 12 hours, the mixture is filtered with a 0.22 μm aqueous filter membrane, and washed with deionized water for several times to remove excess PDDA, and the microspheres on the aqueous filter membrane are dispersed again in deionized water to obtain a positively charged microsphere dispersion;

[0224] Preparation of single-layer MXene solution: Dissolve multilayer MXene powder in water, and under the protection of inert gas, ultrasonicate for 40 minutes to destroy the multilayer structure. During this period, control the water temperature below 40°C by ice bath or other means to avoid MXene oxidation.

[0225] The MXene dispersion obtained by ultrasound was centrifuged at a high speed of more than 5000 rpm for 10 minutes, and the supernatant was the single-layer MXene solution.

[0226] The concentration of the monolayer MXene solution was determined by vacuum filtration of the film and adjusted to 1 mg / ml.

[0227] The microsphere dispersion was added dropwise to the monolayer MXene solution for electrostatic self-assembly. The mass ratio of PMMA microspheres to MXene should be 1:2. The MXene / PMMA microsphere dispersion was slowly stirred for 20 minutes. During the stirring process, the negatively charged MXene nanosheets were spontaneously wrapped on the surface of the PMMA microspheres through electrostatic self-assembly. The prepared MXene / PMMA microsphere ink was further concentrated using high-speed centrifugation (6000 rpm, 20 minutes); the average diameter of the microspheres should be controlled at 0.5-2 microns.

[0228] S2 prepares the sensing layer;

[0229] S3 flexible electrode film preparation

[0230] The flexible film is used as a substrate, and the obtained flexible substrate is evenly sprayed with photoresist. The flexible film with photoresist is dried on a constant temperature heating table at 80°C for 30 minutes to cure the photoresist.

[0231] Using an inkjet printer to print a desired interdigital electrode pattern on a film as a mask;

[0232] Place the pattern surface of the mask close to the cured photoresist coating, expose to ultraviolet light for 3 minutes, and use a developer to soak and remove the photoresist on the patterned part;

[0233] After the sample was plasma cleaned with argon and oxygen, titanium layer, copper layer, and gold layer were magnetron sputtered on the surface in sequence;

[0234] The remaining photoresist and the metal layer thereon are removed by a release agent to obtain a patterned interdigital electrode layer.

[0235] Wherein, the material of the flexible film is polyethylene terephthalate (PET)

[0236] S4 Assembly

[0237] Use copper wire to connect the two electrodes of the interdigital electrode through conductive silver paste to establish an external circuit. Coat PDMS on the top layer as a fixative, treat the flexible substrate and the sensing layer and flexible electrode film obtained in the above steps with oxygen plasma, and vertically plane-laminate in the order of encapsulation layer-electrode layer-sensing layer-flexible substrate-encapsulation layer. Use the flexible film as the encapsulation layer to assemble the above components into a flexible sensor.

[0238] Comparative Example 5

[0239] The sensor layer in this comparative example is only a single MXene material, has no internal mesoporous structure and no nanowires are deposited on the surface. The remaining steps and parameters are the same as those in Example 2.

[0240] Comparative Example 6

[0241] The sensor layer in this comparative example is only a mesoporous structure MXene sensing layer, and no nanowires are deposited on the surface. The remaining steps and parameters are the same as those in Example 2.

[0242] The water drop contact angle test was performed on the surface treated PDMS of the above embodiments and comparative examples 1-4. The water drop contact optical images are shown in FIG. Figure 4 As shown, the lower the water droplet contact angle, the higher the surface energy of the interface, that is, the better the hydrophilicity. The contact angle of the PDMS after the co-treatment in Example 2 (21.67±2.08°) is much lower than the contact angle of the untreated PDMS in Comparative Example 1 (102±4.58°). It can be seen that the co-treated PDMS surface in Example 2 has good hydrophilicity. Figure 5 The figure is a graph showing the change of the water drop contact angle over time on the PDMS surface after different surface treatment methods in Example 2 and Comparative Examples 1-4. It can be seen that the hydrophilic effect of the PDMS surface treated in Example 2 can last for a long time. The PDMS treated with oxygen plasma in Comparative Example 2 also shows good hydrophilicity (14±6.56°), but this hydrophilic modification is not long-lasting, and the contact angle recovers to 93.67±4.04° after only 6 hours. In contrast, the PDMS treated in Example 2 has long-term and stable hydrophilicity, and the surface contact angle remains at 29.67±4.62° after 48 hours. A good hydrophilic surface helps the uniform deposition of the conductive ink solution, and the durability of the surface modification avoids the strict time requirements between process steps, thereby improving process flexibility.

[0243] For the above-mentioned Example 2 and Comparative Examples 1-4, the PDMS and the sensing layer obtained by the surface treatment process were subjected to adhesion tests, and the data were processed and calculated. The interfacial adhesion strength of the embodiment was dozens of times that of the adhesion strength of Comparative Example 1, and was also significantly improved compared to Comparative Examples 2-4, indicating the mechanical stability of the sensing layer of the present invention.

[0244] The above-mentioned adhesion strength test method is specifically as follows: adhere the 3M tape for test to the ink coating surface to be tested, the sample size is 10 mm long and 10 mm wide, and a block roller with constant pressure is used for rolling. After leaving it for 5 minutes, a tensile testing machine is used to test the adhesion strength by stretching it in the vertical direction, and the adhesion strength is calculated based on the maximum tensile force and the sample size.

[0245] The above-mentioned Example 2 and Comparative Examples 5-6 were tested for the sensitive response of the sensor, and the data were normalized. The pressure current response curves are shown in FIG. Figure 7By comparing the pressure current response curves of Example 2 and Comparative Examples 5-6, it can be seen that the mesoporous structure and nanowire deposition in Example 2 effectively improve the sensitive response range and saturation threshold of the sensing layer, that is, the sensitivity and detection range of the sensor device prepared by the present invention are improved.

[0246] For the above-mentioned Example 2 and Comparative Example 6, a four-probe square resistance test of the sensing layer was performed, and the curve of the square resistance value changing with time is as follows: Figure 8 As shown. By comparing the test values ​​of Example 2 and Comparative Example 6, it can be seen that the deposition process of metal nanowires increases the conductive layer area of ​​the sensing layer and effectively reduces the interfacial resistance of the sensing layer. Secondly, since the metal nanowires prepared by the chemical self-assembly process can grow and penetrate into the sub-surface layer of the MXene coating to form a network structure, the contact between MXene and air and water is reduced, the oxidation of MXene is slowed down, and the stability of the device is effectively improved.

[0247] The lamellar structure of MXene and the rich functional groups on the surface of MXene nanosheets make the MXene coating obtained by electrodeposition present a stacked state inside. MXene is a material with good electrical conductivity that can form a conductive network. When subjected to external pressure, the flexible substrate will deform, and this deformation will be transmitted to the MXene coating. The deformation of the MXene layer will cause the distance between the MXenes to change, thereby changing the charge transfer path and impedance. Furthermore, under a large pressure load, the mesoporous structure reinforced by the coating microspheres deforms, expanding the conduction path, so that under a large pressure load, the overall performance is a high sensitivity response under large pressure. And because the internal mesoporous structure of the functional layer is reinforced by microspheres, the stacking of MXene nanosheets is improved. After the load is removed, the deformed structure can recover quickly, improving the overall signal response and force stability of the system.

[0248] Therefore, the present invention provides a sensing layer and a preparation method, a sensor made of the sensing layer and a preparation method thereof, which solves the problems in the prior art of poor adhesion, poor detection accuracy, weak stability and durability, poor flexibility and mechanical properties, and small sensitivity and detection range.

[0249] In the description of this specification, the description with reference to the terms "an experimental example", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the experimental example or example are included in at least one experimental example or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same experimental example or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more experimental examples or examples in a suitable manner.

[0250] Finally, it should be noted that the above experimental examples are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred experimental examples, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for preparing a sensing layer, characterized in that: The method comprises the following preparation steps: S1. Treating the flexible substrate: spin coating the PDMS mixture on the carrier plate, then degreasing, drying, dehydrating, bombarding the PDMS surface with inert gas high-energy plasma, cleaning the obtained PDMS flexible substrate with oxygen plasma, obtaining a hydroxylated PDMS flexible substrate, dipping the hydroxylated PDMS flexible substrate in a PVA solution, drying and then heating, repeating the dipping-drying steps multiple times to obtain a treated PDMS flexible substrate; S2. Modify the treated PDMS flexible substrate to prepare a surface metal layer.

2. The method for preparing a sensing layer according to claim 1, characterized in that: The PDMS mixture liquid adopts a PDMS main agent and a hardener with a mass ratio of 9-11:1, and the bubbles in the mixture liquid are floated to the surface and broken by vacuuming; the spin coating speed of the PDMS mixture liquid is 40-60rpm, the spin coating time is 1-5 minutes, and the carrier plate is spin-coated with the PDMS mixture liquid and dried and hardened in an oven for 1-5 hours; when the PDMS surface is bombarded with inert gas high-energy plasma, the bombardment conditions are: nitrogen / argon flow rate is 50-120sccm, vacuum pressure is 0.6-0.8mbar, power is 200-400w, and bombardment time is 8-12 minutes; the obtained PDMS flexible substrate is cleaned by oxygen plasma The cleaning conditions are: oxygen flow rate of 50-100sccm, pressure of 0.6-0.8mbar, power of 100w, 1-7 minutes; PVA solution mass fraction of 0.5-2wt%, when preparing PVA solution, PVA is added to pure water and stirred at room temperature for 30-50 minutes, heated to 90-120℃ and stirred for 30-50 minutes, finally, stirred at 50-70℃ for more than 12 hours, the immersion time of hydroxylated PDMS flexible substrate in PVA solution is 8-13 minutes, and the specific process of heating after drying is: after drying with nitrogen, heating on a hot plate at 100-120℃ for 10-20 minutes.

3. The method for preparing a sensing layer according to claim 1, characterized in that: The specific steps of S2 are: spraying MXene / microsphere ink onto the treated surface of PDMS flexible substrate, pyrolyzing the PDMS flexible substrate with MXene / microsphere coating to remove the microspheres after spraying, and obtaining a flexible substrate with mesoporous MXene film deposited, and then placing the flexible substrate with mesoporous MXene film deposited in a solution of metal ions, growing metal nanowires on the MXene coating, and obtaining a surface metal layer.

4. The method for preparing a sensing layer according to claim 3, characterized in that: During the spraying process, ensure that the water in the MXene / microsphere ink evaporates before each spraying, and spray multiple times until the MXene / microsphere deposition amount is about 0.1-0.3mg / cm 2 The steps of pyrolysis to remove microspheres are as follows: after spraying, the PDMS flexible substrate with MXene / microsphere coating is placed in a drying oven to dry, and then pyrolysis is performed in a vacuum sintering furnace to remove the microspheres. Under the protection of inert gas, the pyrolysis treatment is performed at a high temperature of 350-500°C for 13-20 minutes to burst the microspheres inside the coating, leaving hollow holes inside. Before high-temperature pyrolysis, the vacuum sintering furnace is repeatedly filled with inert gas to exclude oxygen. The heating temperature of the vacuum sintering furnace is controlled at above 100°C / minute to prevent the microspheres from melting due to heat.

5. A sensing layer made according to the method for preparing a sensing layer according to any one of claims 1 to 4.

6. A sensor, characterized in that: A sensing layer prepared by the method for preparing a sensing layer according to any one of claims 1 to 4.

7. The method for preparing a sensor according to claim 6, characterized in that: The method comprises the following preparation steps: S1. prepare a microsphere dispersion and a MXene solution respectively, add the microsphere dispersion dropwise into the MXene solution for electrostatic self-assembly, slowly stir the mixed MXene / microsphere dispersion, during which the negatively charged MXene nanosheets are wrapped on the surface of the microspheres by electrostatic self-assembly, and concentrate after stirring to obtain the MXene / microsphere ink to be prepared; S2. Prepare the sensing layer; S3. Preparation of a flexible electrode film: using a flexible film as a substrate, spraying a photoresist evenly on the obtained flexible substrate, drying and curing the photoresist on the flexible film with the photoresist, and printing the desired interdigitated electrode pattern on a film as a mask using an inkjet printer; The pattern surface of the mask is placed close to the cured photoresist coating, and after ultraviolet exposure, the photoresist of the pattern part is removed; After the obtained sample was plasma cleaned with argon and oxygen, a titanium layer, a copper layer, and a gold layer were magnetron sputtered on the surface in sequence; Removing the remaining photoresist and the metal layer thereon by a release agent to obtain a patterned interdigital electrode layer; S4. Assembly: Use copper wire to connect the two electrodes of the interdigital electrode through conductive silver paste to establish an external circuit, apply PDMS on the top layer as a fixing agent, treat the flexible substrate and the sensing layer and flexible electrode film obtained in the above steps with oxygen plasma, and vertically plane-laminate in the order of encapsulation layer - electrode layer - sensing layer - flexible substrate - encapsulation layer; the encapsulation layer is a flexible film.

8. The sensor according to claim 7, characterized in that The specific steps for preparing the microsphere dispersion are as follows: dispersing the prepared microsphere solution in a cationic polymer polydiallyl dimethyl ammonium chloride solution PDDA by ultrasonic treatment to obtain a mixture, stirring the mixture, filtering it with an aqueous filter membrane, and washing it with deionized water to remove the cationic polymer polydiallyl dimethyl ammonium chloride solution PDDA, and re-dispersing the microspheres on the aqueous filter membrane in deionized water to obtain a positively charged microsphere dispersion; the specific steps for preparing the MXene solution are as follows: dissolving the MXene powder in water, ultrasonicating it for 20-40 minutes under the protection of an inert gas to obtain a MXene dispersion, and then centrifuging the MXene dispersion to obtain the supernatant, which is the MXene solution.

9. The sensor according to claim 7, characterized in that The microspheres are one or more of polystyrene microspheres, polymethyl methacrylate microspheres, polystyrene-co-acrylate copolymer microspheres, and polylactic acid microspheres, and the average diameter of the microspheres is 0.5-2 microns.

10. The sensor according to claim 7, characterized in that In the step S1, during electrostatic self-assembly, the mass ratio of microspheres to MXene is 1:2; the material of the flexible film in the step S3 and the step S4 is a flexible insulating material, which is one or more of polyimide, polyethylene terephthalate, polyethylene naphthalate, polymethyl methacrylate and polyurethane; preferably, the flexible film is polyimide.

Citation Information

Patent Citations

  • MXene-material-based flexible strain sensor

    CN108168420A

  • High-sensitivity flexible piezoresistive sensor based on MXene bionic skin structure

    CN110579297A

  • Preparation method of silver nanowire / MXene flexible stress sensor

    CN110864828A

  • Preparation method of wearable transparent flexible film type strain sensor

    CN111141427A

  • Flexible pressure sensor based on ink / MXene composite film and preparation method thereof

    CN115165168A