In-situ measurement method for wetting angle of liquid brazing filler metal

The in-situ measurement method addresses human error and characterizes the dynamic solder wetting process by using a tube furnace and high-speed camera, ensuring accurate and real-time solder angle assessment.

CN119086357APending Publication Date: 2024-12-06CHINA ELECTRONIC TECH GRP CORP NO 38 RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411221734.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Current solder wetting angle measurement methods suffer from human errors in metallographic polishing and cannot characterize the dynamic wetting process under actual working conditions.

Method used

An in-situ measurement method involving substrate preparation, use of a tube furnace with inert gas or evacuation, and high-speed camera imaging to capture the solder's dynamic wetting angle on any substrate and at different temperatures.

Benefits of technology

The method provides accurate, real-time measurement of the solder's wetting angle, reducing errors and enabling characterization of the dynamic process across various substrates and conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119086357A_ABST
    Figure CN119086357A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of electronic packaging, in particular to an in-situ measurement method for a wetting angle of liquid brazing filler metal, which comprises the following steps of: placing a brazing filler metal body to be measured right above a substrate to be measured by using a means which is the same as that of operating a tubular furnace for heating, adjusting the view of an external high-speed camera to be horizontal with the substrate, heating after setting the temperature, and measuring the wetting angle of the brazing filler metal body to be measured; and heating until the brazing filler metal body is completely dissolved so as to measure the wetting angle. According to the invention, the in-situ measurement of the dynamic wetting angle of the brazing filler metal on any substrate under different temperature curves and atmospheres can be realized. Compared with other wetting angle measuring methods, the method does not need professional equipment, and is simple to operate, wide in application range and higher in accuracy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electronic packaging, and in particular to an in-situ measurement method of a liquid solder wetting angle. Background Art

[0002] The wetting angle is an important indicator for characterizing wetting performance. It refers to the angle between the liquid-solid surface and the tangent line of the liquid surface at the liquid-solid-gas interface between the fluid droplet and the solid substrate. For the solder and the substrate to be soldered, the smaller the wetting angle between the two, the better the wetting performance, and more effective welding can be achieved. Therefore, measuring the wetting angle between the substrate and different solders under specific conditions can provide an important reference for the selection of solder.

[0003] The commonly used method for measuring the solder wetting angle is limited to directly preparing the sample under air conditions, obtaining the cross-sectional image of the droplet after metallographic polishing, and then measuring the wetting angle. The above method has many limitations. There are human errors in the metallographic polishing process, which affects the accuracy and cannot characterize the dynamic wetting process of the solder. At the same time, affected by the actual working conditions, it is necessary to characterize the dynamic wetting process of the solder under different substrates, temperature curves and atmospheres.

[0004] In view of the above-mentioned defects, the inventors of the present invention finally obtained the present invention after a long period of research and practice. Summary of the invention

[0005] The purpose of the present invention is to solve the problem that the currently commonly used solder wetting angle measurement method has human errors in the metallographic polishing process, which affects the accuracy and cannot characterize the dynamic wetting process of the solder, and provides an in-situ measurement method for the wetting angle of liquid solder.

[0006] In order to achieve the above object, the present invention discloses an in-situ measurement method of a liquid solder wetting angle, comprising the following steps:

[0007] S1, polish the substrate to be tested, remove the oxides and organic matter on the surface of the solder to be tested and the substrate, ultrasonically clean the solder to be tested and the substrate, and blow dry.

[0008] S2, placing the brazing material in the center of the substrate, transferring it into the tube furnace, setting the temperature curve of the tube furnace, and adjusting the camera position of the external high-speed camera;

[0009] S3, heating the tube furnace, filling it with inert gas or evacuating it, so that the brazing material is dissolved and spread on the substrate;

[0010] S4, obtaining the solder image of the whole process in step S3, and statistically identifying the wetting angle through computer.

[0011] In the step S1, the roughness of the sandpaper used to polish the substrate is 400# to 5000#.

[0012] In the step S1, acetone is used to remove oxides and organic matter on the surface of the solder to be tested and the substrate.

[0013] In the step S1, the solder to be tested and the substrate are ultrasonically cleaned with a mixture of ethanol and acetone and pure water for 5 minutes, and finally dried with nitrogen.

[0014] In step S2, the field of view of the external high-speed camera needs to be level with the upper surface of the substrate, and an external light source is used to keep the field of view clear.

[0015] In the step S2, the type of inert gas introduced is specified according to the protective gas used in reflow soldering in industrial production, which is generally nitrogen or argon.

[0016] In step S2, sealing valves are respectively provided at both ends of the quartz tube in the tubular furnace, wherein the sealing valve at one end is connected to the vacuum pump and the gas cylinder through a gas interface, and a glass lens is embedded in the sealing valve at the other end.

[0017] Compared with the prior art, the beneficial effect of the present invention is that the present invention can realize the in-situ measurement of the dynamic wetting angle of the solder on any substrate and at different temperatures. Compared with other wetting angle measurement methods, the present method is simple to operate, has a wide range of applications, and is more accurate. In order to reduce the error caused by the volume of the solder, the present invention can select raw materials of different specifications and sizes for testing, repeatedly test the in-situ measurement value of the dynamic wetting angle, and minimize the error caused by the experimental parameters. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 A schematic diagram of the appearance of an embodiment of the present invention;

[0019] Figure 2 It is a structural schematic diagram of an embodiment of the present invention;

[0020] Figure 3 The figure is a schematic diagram of a camera adjustment method and a light source setting in an embodiment of the present invention.

[0021] Figure 4 This is an image of the in-situ change of the wetting angle in an embodiment of the present invention.

[0022] The numbers in the figure represent:

[0023] 1-tube furnace body; 2-solder to be tested; 3-substrate to be tested; 4-gas interface; 5-sealing valve; 6-glass lens; 7-reflecting prism; 8-light source; 9-semi-mirror. DETAILED DESCRIPTION

[0024] The above and other technical features and advantages of the present invention are described in more detail below in conjunction with the accompanying drawings.

[0025] Example 1

[0026] A method for in-situ measurement of a liquid solder wetting angle comprises the following steps:

[0027] S1, polish the substrate to be tested, remove the oxides and organic matter on the surface of the solder to be tested and the substrate, ultrasonically clean the solder to be tested and the substrate, and blow dry.

[0028] S2, placing the brazing material in the center of the substrate, transferring it into the tube furnace, setting the temperature curve of the tube furnace, and adjusting the camera position of the external high-speed camera;

[0029] S3, heating the tube furnace, filling it with inert gas or evacuating it, so that the brazing material is dissolved and spread on the substrate;

[0030] S4, obtaining the solder image of the whole process in step S3, and statistically identifying the wetting angle through computer.

[0031] Example 2

[0032] A device for in-situ measurement of the wetting angle of liquid solder includes a tube furnace body 1, a gas interface 4 and a high-speed camera. The solder 2 to be tested and the substrate 3 to be tested are placed at the center of the tube furnace body 1. A sealing valve is installed at each end of the quartz tube. One end is connected to a vacuum pump and a gas cylinder through a gas interface, and a glass lens 6 is embedded in the sealing valve 5 at the other end to achieve transparent sealing. Figure 2 As shown, during operation, remove the sealing valve at the left end, put in the sample and seal it. Connect the vacuum pump through the gas interface, evacuate and fill with inert gas, repeat the operation several times to make the inside of the quartz tube full of inert gas. Then, adjust the experimental parameters and set the position of the high-speed camera to start the experiment.

[0033] During operation, the sample heating temperature is regulated by setting the temperature curve of the tube furnace body 1. The furnace body 1 is connected to a gas cylinder or a vacuum pump through a gas interface 4, and the conditions required for the experiment are input. A high-speed camera is set at the other end of the tube furnace body 1 to shoot the dynamic changes of the brazing material wetting angle with the assistance of a light source. The high-speed camera is connected to a computer, and the contact angle is calculated in real time by computer software.

[0034] High-speed camera adjustment method and light source setting Figure 3 As shown: Turn on the light source 8 in the tube furnace, and the light is reflected by the half mirror and then directed to the surface of the sample to be tested. The reflecting prism 7 at the end of the tube furnace reflects the light twice, so that it passes through the half mirror 9 again and immerses into the high-speed camera. The arrow shows the light path. Adjust the camera position until the center of the field of view is the sample to be tested.

[0035] Example 3

[0036] This example uses tin-lead eutectic solder with a size of Cylindrical sample; the substrate to be soldered is a PCB substrate with nickel-gold plating. In order to simulate the nitrogen reflow process in industrial production, it is necessary to measure the wetting angle of the nitrogen atmosphere under specific reflow temperature parameters. The temperature curve adjustment module provided by the tube furnace can be used to input the reflow curve. The advantage of the tube furnace is that the sample is heated evenly, avoiding the error caused by unidirectional heating methods such as hot plates. Use 2000# and 5000# sandpaper to polish the surface of the substrate to be soldered, and put them in acetone to clean the surface grease, and then use ethanol acetone mixture and pure water ultrasonic cleaning for 5 minutes, and finally use nitrogen to blow dry.

[0037] Place the brazing material at the center of the substrate and transfer the two to a tube furnace, where nitrogen is continuously introduced for 10 minutes. The parameters of the tube furnace are a heating rate of 10°C / min and a peak temperature of 210°C. Adjust the high-speed camera so that the field of view is level with the substrate surface.

[0038] Turn on the tube furnace and high-speed camera, and observe that the solder gradually melts and spreads on the surface of the substrate to be tested. The high-speed camera captures the dynamic changes in the wetting angle of the liquid solder, and realizes the in-situ measurement of the wetting angle of the solder. The wetting angle change image captured by the high-speed camera during the measurement process is shown in the figure below. Figure 4 shown.

[0039] The above description is only a preferred embodiment of the present invention, which is only illustrative and not restrictive of the present invention. Those skilled in the art understand that many changes, modifications, and even equivalences may be made to the present invention within the spirit and scope defined by the claims of the present invention, but all of them will fall within the scope of protection of the present invention.

Claims

1. An in-situ measurement method of a liquid solder wetting angle, characterized in that: The following steps are involved: S1, polish the substrate to be tested, remove the oxides and organic matter on the surface of the solder to be tested and the substrate, ultrasonically clean the solder to be tested and the substrate, and blow dry. S2, placing the brazing material in the center of the substrate, transferring it into the tube furnace, setting the temperature curve of the tube furnace, and adjusting the camera position of the external high-speed camera; S3, heating the tube furnace, filling it with inert gas or evacuating it, so that the brazing material is dissolved and spread on the substrate; S4, obtaining the solder image of the whole process in step S3, and statistically identifying the wetting angle through computer.

2. The in-situ measurement method of the wetting angle of liquid solder according to claim 1, characterized in that: In the step S1, the roughness of the sandpaper used to polish the substrate is 400# to 5000#.

3. The in-situ measurement method of the wetting angle of liquid solder according to claim 1, characterized in that: In the step S1, acetone is used to remove oxides and organic matter on the surface of the solder to be tested and the substrate.

4. The in-situ measurement method of the wetting angle of liquid solder according to claim 1, characterized in that: In the step S1, the solder to be tested and the substrate are ultrasonically cleaned with a mixture of ethanol and acetone and pure water for 5 minutes, and finally dried with nitrogen.

5. The in-situ measurement method of the wetting angle of liquid solder according to claim 1, characterized in that: In step S2, the field of view of the external high-speed camera needs to be level with the upper surface of the substrate, and an external light source is used to keep the field of view clear.

6. The in-situ measurement method of the liquid solder wetting angle according to claim 1, characterized in that: In step S2, the inert gas is nitrogen or argon.

7. The in-situ measurement method of the wetting angle of liquid solder according to claim 1, characterized in that: In step S2, sealing valves are respectively provided at both ends of the quartz tube in the tubular furnace, wherein the sealing valve at one end is connected to the vacuum pump and the gas cylinder through a gas interface, and a glass lens is embedded in the sealing valve at the other end.